General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.84 g/cm³ Show Material materials with Densidad of 2.84 g/cm³ | T87 | AA Standards, ASTM B209 |
2.84 g/cm³ Show Material materials with Densidad of 2.84 g/cm³ | T87 | ||
3.1 g/cm³ Show Material materials with Densidad of 3.1 g/cm³ | T87 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 105.0 MPa Show Material materials with Bending Fatigue Strength of 105.0 MPa | T87 | AA Standards | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | |||
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | T87 | AA Standards, ASTM B209 | A100 | |
3.0 % Show Material materials with Elongación of 3.0 % | T87 | AA Standards, ASTM B209 | A100 | ||
5.0 % Show Material materials with Elongación of 5.0 % | T87 | AA Standards, ASTM B209 | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | T87 | AA Standards, ASTM B209 | A100 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T87 | AA Standards, ASTM B209 | A50 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T87 | AA Standards, ASTM B209 | A100 | ||
7.0 % Show Material materials with Elongación of 7.0 % | T87 | AA Standards, ASTM B209 | A50 | ||
7.4 % Show Material materials with Elongación of 7.4 % | T87 | ||||
10.0 % Show Material materials with Elongación of 10.0 % | T87 | AA Standards | A50 | ||
10 % Show Material materials with Elongación of 10 % | T87 | ||||
Límite elástico | 340.0 MPa Show Material materials with Límite elástico of 340.0 MPa | T87 | AA Standards, ASTM B209 | RP02 | |
345.0 MPa Show Material materials with Límite elástico of 345.0 MPa | T87 | AA Standards, ASTM B209 | RP02 | ||
350.0 MPa Show Material materials with Límite elástico of 350.0 MPa | T87 | AA Standards, ASTM B209 | RP02 | ||
360.0 MPa Show Material materials with Límite elástico of 360.0 MPa | T87 | AA Standards, ASTM B209 | RP02 | ||
395.0 MPa Show Material materials with Límite elástico of 395.0 MPa | T87 | AA Standards | RP02 | ||
395 MPa Show Material materials with Límite elástico of 395 MPa | T87 | RP02 | |||
400.0 MPa Show Material materials with Límite elástico of 400.0 MPa | T87 | ||||
Módulo de cizallamiento | 26.0 GPa Show Material materials with Módulo de cizallamiento of 26.0 GPa | T87 | |||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T87 | AA Standards, ASTM B209 | ||
73 GPa Show Material materials with Módulo elástico of 73 GPa | T87 | ||||
74.0 GPa Show Material materials with Módulo elástico of 74.0 GPa | T87 | ||||
Plane-Strain Fracture Toughnes | -196 °C | 38.9 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 38.9 MPa·√m | T87 | For plate in T-L direction | |
24 °C | 30.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.8 MPa·√m | T87 | For plate in T-L direction | ||
Resistencia a la fatiga | 103 MPa Show Material materials with Resistencia a la fatiga of 103 MPa | T87 | for 5x10⁸ cycles | ||
Resistencia a la fluencia | 24 °C | 420 MPa Show Material materials with Resistencia a la fluencia of 420 MPa | T87 | up to 1000 hours | |
100 °C | 315 MPa Show Material materials with Resistencia a la fluencia of 315 MPa | T87 | up to 1000 hours | ||
150 °C | 235 MPa Show Material materials with Resistencia a la fluencia of 235 MPa | T87 | up to 1000 hours | ||
205 °C | 150 MPa Show Material materials with Resistencia a la fluencia of 150 MPa | T87 | up to 1000 hours | ||
230 °C | 130 MPa Show Material materials with Resistencia a la fluencia of 130 MPa | T87 | up to 1000 hours | ||
260 °C | 105 MPa Show Material materials with Resistencia a la fluencia of 105 MPa | T87 | up to 1000 hours | ||
270 °C | 17 MPa Show Material materials with Resistencia a la fluencia of 17 MPa | T87 | up to 1000 hours | ||
315 °C | 34 MPa Show Material materials with Resistencia a la fluencia of 34 MPa | T87 | up to 1000 hours | ||
Resistencia a la tracción | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T87 | AA Standards, ASTM B209 | ||
425.0 MPa Show Material materials with Resistencia a la tracción of 425.0 MPa | T87 | AA Standards, ASTM B209 | |||
440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T87 | AA Standards, ASTM B209 | |||
475.0 MPa Show Material materials with Resistencia a la tracción of 475.0 MPa | T87 | AA Standards | |||
475 MPa Show Material materials with Resistencia a la tracción of 475 MPa | T87 | ||||
480.0 MPa Show Material materials with Resistencia a la tracción of 480.0 MPa | T87 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 860.0 J/(kg·K) Show Material materials with Calor específico of 860.0 J/(kg·K) | T87 | ||
Coeficiente de dilatación térmica | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | T87 | ||
20 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | T87 | AA Standards, ASTM B209 | |
100 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | T87 | AA Standards, ASTM B209 | |
Conductividad térmica | 113.0 - 172.0 W/(m·K) Show Material materials with Conductividad térmica of 113.0 - 172.0 W/(m·K) | T87 | AA Standards, ASTM B209 | |
120.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 W/(m·K) | T87 | |||
Temperatura de fusión | 540.0 °C Show Material materials with Temperatura de fusión of 540.0 °C | T87 | ||
545.0 - 645.0 °C Show Material materials with Temperatura de fusión of 545.0 - 645.0 °C | T87 | AA Standards, ASTM B209 |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 16000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 26000000.0 S/m | T87 | AA Standards, ASTM B209 | |
17000000 S/m Show Material materials with Conductividad eléctrica of 17000000 S/m | T87 | Typical/derived value | ||
Resistividad eléctrica | 3.85e-08 - 6.25e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 - 6.25e-08 Ω·m | T87 | AA Standards, ASTM B209 | |
5.7e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.7e-08 Ω·m | T87 | Typical value | ||
Specific Electrical conductivity | 30.0 % IACS Show Material materials with Specific Electrical conductivity of 30.0 % IACS | T87 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 91.5 - 93.8 % Show Material materials with Aluminio of 91.5 - 93.8 % | T87 | |
Circonio | 0.1 - 0.25 % Show Material materials with Circonio of 0.1 - 0.25 % | T87 | AA Standards, ASTM B209 |
Cobre | 5.8 - 6.8 % Show Material materials with Cobre of 5.8 - 6.8 % | T87 | AA Standards, ASTM B209 |
Hierro | 0.30 % Show Material materials with Hierro of 0.30 % | T87 | AA Standards, ASTM B209 |
0.3 % Show Material materials with Hierro of 0.3 % | T87 | ||
Magnesio | 0.02 % Show Material materials with Magnesio of 0.02 % | T87 | AA Standards, ASTM B209 |
Manganeso | 0.2 - 0.4 % Show Material materials with Manganeso of 0.2 - 0.4 % | T87 | AA Standards, ASTM B209 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T87 | |
Silicona | 0.2 % Show Material materials with Silicona of 0.2 % | T87 | AA Standards, ASTM B209 |
Titanio | 0.02 - 0.1 % Show Material materials with Titanio of 0.02 - 0.1 % | T87 | AA Standards, ASTM B209 |
Vanadio | 0.05 - 0.15 % Show Material materials with Vanadio of 0.05 - 0.15 % | T87 | AA Standards, ASTM B209 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | T87 | AA Standards, ASTM B209 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T31, T351, T3510, T3511, T37), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (T81, T851, T8510, T8511), general: sufficient, in principle it should be protected | |
General machinability | General: good to acceptable | |
Workability | general (condition): poor(T31, T351, T3510, T3511), not suitable (T37, T81, T851, T8510, T8511, T87) |