General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H16 | ||
2.8 g/cm³ Show Material materials with Densidad of 2.8 g/cm³ | H16 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 70.0 MPa Show Material materials with Bending Fatigue Strength of 70.0 MPa | H16 | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||
Dureza Brinell | 47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | H16 | AA Standards | |
47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | H16 | 500 kg load, 10 mm ball | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | H16 | AA Standards, ASTM B209 | A50 |
2.0 % Show Material materials with Elongación of 2.0 % | H16 | AA Standards, ASTM B209, ASTM B210 | A50 | |
3.0 % Show Material materials with Elongación of 3.0 % | H16 | AA Standards, ASTM B209, ASTM B313 | A50 | |
4.0 % Show Material materials with Elongación of 4.0 % | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | A50 | |
5.0 % Show Material materials with Elongación of 5.0 % | H16 | AA Standards | A50 | |
5.8 % Show Material materials with Elongación of 5.8 % | H16 | |||
9.5 % Show Material materials with Elongación of 9.5 % | H16 | |||
12.0 % Show Material materials with Elongación of 12.0 % | H16 | AA Standards | A100 | |
Límite elástico | 145.0 MPa Show Material materials with Límite elástico of 145.0 MPa | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | RP02 |
170.0 MPa Show Material materials with Límite elástico of 170.0 MPa | H16 | AA Standards | RP02 | |
170 MPa Show Material materials with Límite elástico of 170 MPa | H16 | RP02 | ||
170.0 MPa Show Material materials with Límite elástico of 170.0 MPa | H16 | |||
Módulo de cizallamiento | 25.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 GPa | H16 | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
69 GPa Show Material materials with Módulo elástico of 69 GPa | H16 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Resistencia a la fatiga | 69 MPa Show Material materials with Resistencia a la fatiga of 69 MPa | H16 | for 5x10⁸ cycles | |
Resistencia a la tracción | 165.0 - 205.0 MPa Show Material materials with Resistencia a la tracción of 165.0 - 205.0 MPa | H16 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
165.0 MPa Show Material materials with Resistencia a la tracción of 165.0 MPa | H16 | AA Standards, ASTM B210, ASTM B211, ASTM B483 | ||
175.0 MPa Show Material materials with Resistencia a la tracción of 175.0 MPa | H16 | AA Standards | ||
180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | H16 | |||
180 MPa Show Material materials with Resistencia a la tracción of 180 MPa | H16 | |||
Resistencia al cizallamiento | 105.0 MPa Show Material materials with Resistencia al cizallamiento of 105.0 MPa | H16 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 890.0 J/(kg·K) Show Material materials with Calor específico of 890.0 J/(kg·K) | H16 | ||
Coeficiente de dilatación térmica | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | H16 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
Conductividad térmica | 159.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 159.0 - 193.0 W/(m·K) | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
180.0 W/(m·K) Show Material materials with Conductividad térmica of 180.0 W/(m·K) | H16 | |||
Temperatura de fusión | 640.0 - 655.0 °C Show Material materials with Temperatura de fusión of 640.0 - 655.0 °C | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
640.0 °C Show Material materials with Temperatura de fusión of 640.0 °C | H16 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 24000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 29000000.0 S/m | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Resistividad eléctrica | 3.45e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 4.17e-08 Ω·m | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 96.8 - 99.0 % Show Material materials with Aluminio of 96.8 - 99.0 % | H16 | |
Cobre | 0.05 - 0.2 % Show Material materials with Cobre of 0.05 - 0.2 % | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
0.7 % Show Material materials with Hierro of 0.7 % | H16 | ||
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H16 | |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H16 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H16, H25) | |
Workability | general (condition): good (O, H12), acceptable (H14, H25), poor(H16, H18) |