General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H36 | ||
2.8 g/cm³ Show Material materials with Densidad of 2.8 g/cm³ | H36 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 110.0 MPa Show Material materials with Bending Fatigue Strength of 110.0 MPa | H36 | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||
Dureza Brinell | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | H36 | AA Standards | |
70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | H36 | 500 kg load, 10 mm ball | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | H36 | AA Standards, ASTM B209 | A50 |
2.0 % Show Material materials with Elongación of 2.0 % | H36 | AA Standards, ASTM B209 | A50 | |
3.0 % Show Material materials with Elongación of 3.0 % | H36 | AA Standards, ASTM B209, ASTM B313 | A50 | |
4.0 % Show Material materials with Elongación of 4.0 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
5.0 % Show Material materials with Elongación of 5.0 % | H36 | AA Standards | A50 | |
5.0 % Show Material materials with Elongación of 5.0 % | H36 | |||
7 % Show Material materials with Elongación of 7 % | H36 | |||
8.0 % Show Material materials with Elongación of 8.0 % | H36 | AA Standards | A100 | |
Límite elástico | 190.0 MPa Show Material materials with Límite elástico of 190.0 MPa | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | RP02 |
220.0 MPa Show Material materials with Límite elástico of 220.0 MPa | H36 | |||
230.0 MPa Show Material materials with Límite elástico of 230.0 MPa | H36 | AA Standards | RP02 | |
230 MPa Show Material materials with Límite elástico of 230 MPa | H36 | RP02 | ||
Módulo de cizallamiento | 25.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 GPa | H36 | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
69 GPa Show Material materials with Módulo elástico of 69 GPa | H36 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Resistencia a la fatiga | 16 MPa Show Material materials with Resistencia a la fatiga of 16 MPa | H36 | for 5x10⁸ cycles | |
Resistencia a la tracción | 240.0 - 285.0 MPa Show Material materials with Resistencia a la tracción of 240.0 - 285.0 MPa | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | H36 | AA Standards | ||
260 MPa Show Material materials with Resistencia a la tracción of 260 MPa | H36 | |||
Resistencia al cizallamiento | 140.0 MPa Show Material materials with Resistencia al cizallamiento of 140.0 MPa | H36 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 890.0 J/(kg·K) Show Material materials with Calor específico of 890.0 J/(kg·K) | H36 | ||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H36 | ||
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
Conductividad térmica | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | H36 | ||
163 W/(m·K) Show Material materials with Conductividad térmica of 163 W/(m·K) | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | ||
Temperatura de fusión | 630.0 - 655.0 °C Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
630.0 °C Show Material materials with Temperatura de fusión of 630.0 °C | H36 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 24000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 S/m | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Resistividad eléctrica | 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.17e-08 Ω·m | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 95.6 - 98.2 % Show Material materials with Aluminio of 95.6 - 98.2 % | H36 | |
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
0.7 % Show Material materials with Hierro of 0.7 % | H36 | ||
Magnesio | 0.8 - 1.3 % Show Material materials with Magnesio of 0.8 - 1.3 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H36 | |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O, H32), sufficient (H34, H36, H38) | |
Workability | general (condition): good (O), acceptable (H32, H34), poor(H36, H38) |