General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H14 | BS EN 573-3, BS EN 485-2 | Sheet |
2.8 g/cm³ Show Material materials with Densidad of 2.8 g/cm³ | H14 |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | |||
Dureza Brinell | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
Elongación | 4.6 % Show Material materials with Elongación of 4.6 % | H14 | |||
Límite elástico | 130.0 MPa Show Material materials with Límite elástico of 130.0 MPa | H14 | |||
Módulo de cizallamiento | 25.0 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 26.0 GPa | Typical for Wrought 3000 Series Aluminium | |||
Módulo elástico | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | H14 | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | |||
Resistencia a la tracción | 140.0 - 180.0 MPa Show Material materials with Resistencia a la tracción of 140.0 - 180.0 MPa | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | H14 |
Aplicaciones térmicas
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Calor específico | 890.0 J/(kg·K) Show Material materials with Calor específico of 890.0 J/(kg·K) | H14 | ||
Coeficiente de dilatación térmica | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | H14 | ||
2.31e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.31e-05 1/K | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
Conductividad térmica | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | H14 | BS EN 573-3, BS EN 485-2 | Sheet |
Temperatura de fusión | 640.0 °C Show Material materials with Temperatura de fusión of 640.0 °C | H14 | ||
655.0 °C Show Material materials with Temperatura de fusión of 655.0 °C | H14 | BS EN 573-3, BS EN 485-2 | Sheet |
Eléctrico
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 29000000.0 S/m | Typical for Wrought 3000 Series Aluminium | |||
Resistividad eléctrica | 4.11e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.11e-08 Ω·m | H14 | BS EN 573-3, BS EN 485-2 | Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminio | 96.3 - 99.1 % Show Material materials with Aluminio of 96.3 - 99.1 % | H14 | |||
Circonio | 0.1 % Show Material materials with Circonio of 0.1 % | H14 | |||
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H14 | |||
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H14 | BS EN 573-3, BS EN 485-2 | Sheet | Total |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | H14 | BS EN 573-3, BS EN 485-2 | Sheet | |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | H14 | BS EN 573-3, BS EN 485-2 | Sheet | Ti + Zr |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H14 | BS EN 573-3, BS EN 485-2 | Sheet |
Technological properties
Property | ||
---|---|---|
Brazing | Very Good | |
General machinability | Acceptable | |
Soldering general | Very Good | |
Welding | Gas: Very Good; Arc: Very Good; Resistance: Good | |
Workability | Cold: Good |