General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H25 | AA Standards, ASTM B209 |
2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H25 | ||
2.8 g/cm³ Show Material materials with Densidad of 2.8 g/cm³ | H25 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | H25 | AA Standards, ASTM B209 | A50 |
4.0 % Show Material materials with Elongación of 4.0 % | H25 | AA Standards, ASTM B209 | A50 | |
6.0 % Show Material materials with Elongación of 6.0 % | H25 | AA Standards, ASTM B209 | A50 | |
6.4 % Show Material materials with Elongación of 6.4 % | H25 | |||
8 % Show Material materials with Elongación of 8 % | H25 | |||
Límite elástico | 130.0 MPa Show Material materials with Límite elástico of 130.0 MPa | H25 | AA Standards, ASTM B209 | RP02 |
160 MPa Show Material materials with Límite elástico of 160 MPa | H25 | RP02 | ||
160.0 MPa Show Material materials with Límite elástico of 160.0 MPa | H25 | |||
Módulo de cizallamiento | 25.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 GPa | H25 | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H25 | AA Standards, ASTM B209 | |
69 GPa Show Material materials with Módulo elástico of 69 GPa | H25 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Resistencia a la tracción | 160.0 MPa Show Material materials with Resistencia a la tracción of 160.0 MPa | H25 | AA Standards, ASTM B209 | |
180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | H25 | |||
180 MPa Show Material materials with Resistencia a la tracción of 180 MPa | H25 | |||
Resistencia al cizallamiento | 105.0 MPa Show Material materials with Resistencia al cizallamiento of 105.0 MPa | H25 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H25 | ||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H25 | ||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H25 | AA Standards, ASTM B209 | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H25 | AA Standards, ASTM B209 | |
Conductividad térmica | 170.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 W/(m·K) | H25 | ||
172 W/(m·K) Show Material materials with Conductividad térmica of 172 W/(m·K) | H25 | AA Standards, ASTM B209 | ||
Temperatura de fusión | 635.0 - 655.0 °C Show Material materials with Temperatura de fusión of 635.0 - 655.0 °C | H25 | AA Standards, ASTM B209 | |
640.0 °C Show Material materials with Temperatura de fusión of 640.0 °C | H25 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 26000000.0 S/m Show Material materials with Conductividad eléctrica of 26000000.0 S/m | H25 | AA Standards, ASTM B209 |
Resistividad eléctrica | 3.85e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 Ω·m | H25 | AA Standards, ASTM B209 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 96.0 - 99.5 % Show Material materials with Aluminio of 96.0 - 99.5 % | H25 | |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | H25 | AA Standards, ASTM B209 |
Cromo | 0.2 % Show Material materials with Cromo of 0.2 % | H25 | AA Standards, ASTM B209 |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | H25 | AA Standards, ASTM B209 |
0.7 % Show Material materials with Hierro of 0.7 % | H25 | ||
Magnesio | 0.2 - 0.8 % Show Material materials with Magnesio of 0.2 - 0.8 % | H25 | AA Standards, ASTM B209 |
Manganeso | 0.3 - 0.8 % Show Material materials with Manganeso of 0.3 - 0.8 % | H25 | AA Standards, ASTM B209 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H25 | |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | H25 | AA Standards, ASTM B209 |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | H25 | AA Standards, ASTM B209 |
Zinc | 0.4 % Show Material materials with Zinc of 0.4 % | H25 | AA Standards, ASTM B209 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H25, H16, H18) | |
Workability | general (condition): good (O), acceptable (H12, H14, H25), poor(H16, H18) |