General
Property | Value | Condition |
---|---|---|
Densidad | 3.0 g/cm³ Show Material materials with Densidad of 3.0 g/cm³ | F |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | F | |||
Compressive yield strength | 131 MPa Show Material materials with Compressive yield strength of 131 MPa | F | |||
Dureza Brinell | 70.0 - 85.0 [-] Show Material materials with Dureza Brinell of 70.0 - 85.0 [-] | F | 500 kg load, 10 mm b | ||
70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
95.0 [-] Show Material materials with Dureza Brinell of 95.0 [-] | F | Pink Sheets, ASTM B108 | Casting | ||
Elongación | 1.5 % Show Material materials with Elongación of 1.5 % | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | A100 |
2 % Show Material materials with Elongación of 2 % | F | Sand cast, elongation in 50 mm | |||
2.1 % Show Material materials with Elongación of 2.1 % | F | ||||
2.5 % Show Material materials with Elongación of 2.5 % | F | Pink Sheets, ASTM B108 | Casting | A100 | |
Límite elástico | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 |
95.0 MPa Show Material materials with Límite elástico of 95.0 MPa | F | Pink Sheets, ASTM B108 | Casting | RP02 | |
110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | F | ||||
124 MPa Show Material materials with Límite elástico of 124 MPa | F | Sand cast, RP02 | |||
Módulo de cizallamiento | 28.0 GPa Show Material materials with Módulo de cizallamiento of 28.0 GPa | F | |||
Módulo elástico | 74 GPa Show Material materials with Módulo elástico of 74 GPa | F | |||
78.0 GPa Show Material materials with Módulo elástico of 78.0 GPa | F | ||||
Resistencia a la fatiga | 70.0 - 83.0 MPa Show Material materials with Resistencia a la fatiga of 70.0 - 83.0 MPa | F | for 5x10⁸ cycles, R.R. Moore type test | ||
Resistencia a la tracción | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | F | |||
160.0 MPa Show Material materials with Resistencia a la tracción of 160.0 MPa | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | F | Pink Sheets, ASTM B108 | Casting | ||
186 MPa Show Material materials with Resistencia a la tracción of 186 MPa | F | Sand cast | |||
Resistencia al cizallamiento | 152 MPa Show Material materials with Resistencia al cizallamiento of 152 MPa | F |
Aplicaciones térmicas
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Calor específico | 860.0 J/(kg·K) Show Material materials with Calor específico of 860.0 J/(kg·K) | F | ||
Coeficiente de dilatación térmica | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | F | ||
Conductividad térmica | 110.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 W/(m·K) | F | ||
Temperatura de fusión | 510.0 - 607.0 °C Show Material materials with Temperatura de fusión of 510.0 - 607.0 °C | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
540.0 °C Show Material materials with Temperatura de fusión of 540.0 °C | F |
Eléctrico
Property | Value | Condition | Comment |
---|---|---|---|
Conductividad eléctrica | 16000000 S/m Show Material materials with Conductividad eléctrica of 16000000 S/m | F | Typical/Derived values |
Resistividad eléctrica | 6.39e-08 Ω·m Show Material materials with Resistividad eléctrica of 6.39e-08 Ω·m | F | Typical values |
Specific Electrical conductivity | 27.0 - 28.0 % IACS Show Material materials with Specific Electrical conductivity of 27.0 - 28.0 % IACS | F | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 85.8 - 91.5 % Show Material materials with Aluminio of 85.8 - 91.5 % | F | ||
Cobre | 3.0 - 4.0 % Show Material materials with Cobre of 3.0 - 4.0 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Hierro | 1.0 % Show Material materials with Hierro of 1.0 % | F | ||
1.00 % Show Material materials with Hierro of 1.00 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting | |
Magnesio | 0.1 % Show Material materials with Magnesio of 0.1 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Níquel | 0.35 % Show Material materials with Níquel of 0.35 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Otro | 0.5 % Show Material materials with Otro of 0.5 % | F | ||
Silicona | 5.5 - 6.5 % Show Material materials with Silicona of 5.5 - 6.5 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Titanio | 0.25 % Show Material materials with Titanio of 0.25 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Zinc | 1.0 % Show Material materials with Zinc of 1.0 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |