General
Property | Value | Condition |
---|---|---|
Densidad | 3.0 g/cm³ Show Material materials with Densidad of 3.0 g/cm³ | T6 |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | T6 | |||
Compressive yield strength | 172.0 - 193.0 MPa Show Material materials with Compressive yield strength of 172.0 - 193.0 MPa | T6 | |||
Dureza Brinell | 80.0 - 95.0 [-] Show Material materials with Dureza Brinell of 80.0 - 95.0 [-] | T6 | 500 kg load, 10 mm b | ||
80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
Elongación | 1.5 - 2.0 % Show Material materials with Elongación of 1.5 - 2.0 % | T6 | Sand cast, elongation in 50 mm | ||
1.5 % Show Material materials with Elongación of 1.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | A100 | |
1.8 % Show Material materials with Elongación of 1.8 % | T6 | ||||
Límite elástico | 140.0 MPa Show Material materials with Límite elástico of 140.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 |
160.0 MPa Show Material materials with Límite elástico of 160.0 MPa | T6 | ||||
164 MPa Show Material materials with Límite elástico of 164 MPa | T6 | Sand cast, RP02 | |||
Módulo de cizallamiento | 28.0 GPa Show Material materials with Módulo de cizallamiento of 28.0 GPa | T6 | |||
Módulo elástico | 74 GPa Show Material materials with Módulo elástico of 74 GPa | T6 | |||
78.0 GPa Show Material materials with Módulo elástico of 78.0 GPa | T6 | ||||
Resistencia a la fatiga | 76.0 - 83.0 MPa Show Material materials with Resistencia a la fatiga of 76.0 - 83.0 MPa | T6 | for 5x10⁸ cycles, R.R. Moore type test | ||
Resistencia a la tracción | 215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | T6 | ||||
250 MPa Show Material materials with Resistencia a la tracción of 250 MPa | T6 | Sand cast | |||
Resistencia al cizallamiento | 200.0 - 220.0 MPa Show Material materials with Resistencia al cizallamiento of 200.0 - 220.0 MPa | T6 |
Aplicaciones térmicas
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Calor específico | 860.0 J/(kg·K) Show Material materials with Calor específico of 860.0 J/(kg·K) | T6 | ||
Coeficiente de dilatación térmica | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T6 | ||
Conductividad térmica | 110.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 W/(m·K) | T6 | ||
Temperatura de fusión | 510.0 - 607.0 °C Show Material materials with Temperatura de fusión of 510.0 - 607.0 °C | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
540.0 °C Show Material materials with Temperatura de fusión of 540.0 °C | T6 |
Eléctrico
Property | Value | Condition | Comment |
---|---|---|---|
Resistividad eléctrica | 6.39e-08 Ω·m Show Material materials with Resistividad eléctrica of 6.39e-08 Ω·m | T6 | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 85.8 - 91.5 % Show Material materials with Aluminio of 85.8 - 91.5 % | T6 | ||
Cobre | 3.0 - 4.0 % Show Material materials with Cobre of 3.0 - 4.0 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Hierro | 1.0 % Show Material materials with Hierro of 1.0 % | T6 | ||
1.00 % Show Material materials with Hierro of 1.00 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Magnesio | 0.1 % Show Material materials with Magnesio of 0.1 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Níquel | 0.35 % Show Material materials with Níquel of 0.35 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Otro | 0.5 % Show Material materials with Otro of 0.5 % | T6 | ||
Silicona | 5.5 - 6.5 % Show Material materials with Silicona of 5.5 - 6.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titanio | 0.25 % Show Material materials with Titanio of 0.25 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Zinc | 1.0 % Show Material materials with Zinc of 1.0 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |