General
Property | Value | Condition |
---|---|---|
Densidad | 2.8 g/cm³ Show Material materials with Densidad of 2.8 g/cm³ | T71 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | T71 | ||||
Compressive yield strength | 248 MPa Show Material materials with Compressive yield strength of 248 MPa | T71 | ||||
Dureza Brinell | 75 [-] Show Material materials with Dureza Brinell of 75 [-] | T71 | 500 kg load, 10 mm b | |||
75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | T71 | Pink Sheets, ASTM B618 | Casting | |||
80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | T71 | Pink Sheets, ASTM B108 | Casting | |||
Elongación | -195 °C | 1.5 % Show Material materials with Elongación of 1.5 % | T71 | Sand cast, elongation in 50 mm | ||
-80 °C | 1.5 % Show Material materials with Elongación of 1.5 % | T71 | Sand cast, elongation in 50 mm | |||
-28 °C | 1.5 % Show Material materials with Elongación of 1.5 % | T71 | Sand cast, elongation in 50 mm | |||
1.5 % Show Material materials with Elongación of 1.5 % | T71 | |||||
24 °C | 1.5 % Show Material materials with Elongación of 1.5 % | T71 | Sand cast, elongation in 50 mm | |||
100 °C | 2 % Show Material materials with Elongación of 2 % | T71 | Sand cast, elongation in 50 mm | |||
150 °C | 3 % Show Material materials with Elongación of 3 % | T71 | Sand cast, elongation in 50 mm | |||
205 °C | 8 % Show Material materials with Elongación of 8 % | T71 | Sand cast, elongation in 50 mm | |||
260 °C | 16 % Show Material materials with Elongación of 16 % | T71 | Sand cast, elongation in 50 mm | |||
315 °C | 36 % Show Material materials with Elongación of 36 % | T71 | Sand cast, elongation in 50 mm | |||
371 °C | 50 % Show Material materials with Elongación of 50 % | T71 | Sand cast, elongation in 50 mm | |||
Límite elástico | -195 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | T71 | Sand cast, RP02 | ||
-80 °C | 220 MPa Show Material materials with Límite elástico of 220 MPa | T71 | Sand cast, RP02 | |||
-28 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | T71 | Sand cast, RP02 | |||
150.0 MPa Show Material materials with Límite elástico of 150.0 MPa | T71 | Pink Sheets, ASTM B618 | Casting | RP02 | ||
185.0 MPa Show Material materials with Límite elástico of 185.0 MPa | T71 | Pink Sheets, ASTM B108 | Casting | RP02 | ||
190.0 MPa Show Material materials with Límite elástico of 190.0 MPa | T71 | |||||
24 °C | 200 MPa Show Material materials with Límite elástico of 200 MPa | T71 | Sand cast, RP02 | |||
100 °C | 193 MPa Show Material materials with Límite elástico of 193 MPa | T71 | Sand cast, RP02 | |||
150 °C | 180 MPa Show Material materials with Límite elástico of 180 MPa | T71 | Sand cast, RP02 | |||
205 °C | 90 MPa Show Material materials with Límite elástico of 90 MPa | T71 | Sand cast, RP02 | |||
260 °C | 35 MPa Show Material materials with Límite elástico of 35 MPa | T71 | Sand cast, RP02 | |||
315 °C | 21 MPa Show Material materials with Límite elástico of 21 MPa | T71 | Sand cast, RP02 | |||
371 °C | 14 MPa Show Material materials with Límite elástico of 14 MPa | T71 | Sand cast, RP02 | |||
Módulo de cizallamiento | 26.2 GPa Show Material materials with Módulo de cizallamiento of 26.2 GPa | T71 | ||||
Módulo elástico | 76.0 GPa Show Material materials with Módulo elástico of 76.0 GPa | T71 | ||||
25 °C | 70.3 GPa Show Material materials with Módulo elástico of 70.3 GPa | T71 | ||||
150 °C | 67.6 GPa Show Material materials with Módulo elástico of 67.6 GPa | T71 | ||||
204 °C | 64.1 GPa Show Material materials with Módulo elástico of 64.1 GPa | T71 | ||||
260 °C | 56.5 GPa Show Material materials with Módulo elástico of 56.5 GPa | T71 | ||||
Resistencia a la fatiga | 70 MPa Show Material materials with Resistencia a la fatiga of 70 MPa | T71 | for 5x10⁸ cycles, R.R. Moore type test | |||
Resistencia a la tracción | -195 °C | 282 MPa Show Material materials with Resistencia a la tracción of 282 MPa | T71 | Sand cast | ||
-80 °C | 255 MPa Show Material materials with Resistencia a la tracción of 255 MPa | T71 | Sand cast | |||
-28 °C | 248 MPa Show Material materials with Resistencia a la tracción of 248 MPa | T71 | Sand cast | |||
200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | T71 | |||||
205.0 MPa Show Material materials with Resistencia a la tracción of 205.0 MPa | T71 | Pink Sheets, ASTM B618 | Casting | |||
235.0 MPa Show Material materials with Resistencia a la tracción of 235.0 MPa | T71 | Pink Sheets, ASTM B108 | Casting | |||
24 °C | 240 MPa Show Material materials with Resistencia a la tracción of 240 MPa | T71 | Sand cast | |||
100 °C | 235 MPa Show Material materials with Resistencia a la tracción of 235 MPa | T71 | Sand cast | |||
150 °C | 207 MPa Show Material materials with Resistencia a la tracción of 207 MPa | T71 | Sand cast | |||
205 °C | 117 MPa Show Material materials with Resistencia a la tracción of 117 MPa | T71 | Sand cast | |||
260 °C | 67 MPa Show Material materials with Resistencia a la tracción of 67 MPa | T71 | Sand cast | |||
315 °C | 41 MPa Show Material materials with Resistencia a la tracción of 41 MPa | T71 | Sand cast | |||
371 °C | 25 MPa Show Material materials with Resistencia a la tracción of 25 MPa | T71 | Sand cast | |||
Resistencia al cizallamiento | 241 MPa Show Material materials with Resistencia al cizallamiento of 241 MPa | T71 |
Aplicaciones térmicas
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Calor específico | 880.0 J/(kg·K) Show Material materials with Calor específico of 880.0 J/(kg·K) | T71 | ||
Coeficiente de dilatación térmica | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T71 | ||
Conductividad térmica | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | T71 | ||
Temperatura de fusión | 546.0 - 621.0 °C Show Material materials with Temperatura de fusión of 546.0 - 621.0 °C | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
560.0 °C Show Material materials with Temperatura de fusión of 560.0 °C | T71 |
Eléctrico
Property | Value | Condition | Comment |
---|---|---|---|
Conductividad eléctrica | 20880000 S/m Show Material materials with Conductividad eléctrica of 20880000 S/m | T71 | Typical/Derived values |
Specific Electrical conductivity | 36 % IACS Show Material materials with Specific Electrical conductivity of 36 % IACS | T71 | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 90.3 - 94.1 % Show Material materials with Aluminio of 90.3 - 94.1 % | T71 | ||
Cobre | 1.0 - 1.5 % Show Material materials with Cobre of 1.0 - 1.5 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Hierro | 0.6 % Show Material materials with Hierro of 0.6 % | T71 | ||
0.60 % Show Material materials with Hierro of 0.60 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting | |
Magnesio | 0.4 - 0.6 % Show Material materials with Magnesio of 0.4 - 0.6 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T71 | ||
Silicona | 4.5 - 5.5 % Show Material materials with Silicona of 4.5 - 5.5 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Titanio | 0.25 % Show Material materials with Titanio of 0.25 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Zinc | 0.35 % Show Material materials with Zinc of 0.35 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |