General
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Dureza Brinell | 28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | O | AA Standards | |
28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | O | 500 kg load, 10 mm ball | ||
Elongación | 12.0 % Show Material materials with Elongación of 12.0 % | O | AA Standards, ASTM B209 | A50 |
16.0 % Show Material materials with Elongación of 16.0 % | O | AA Standards, ASTM B209 | A50 | |
19.0 % Show Material materials with Elongación of 19.0 % | O | AA Standards, ASTM B209 | A50 | |
20.0 % Show Material materials with Elongación of 20.0 % | O | AA Standards, ASTM B209 | A100 | |
21.0 % Show Material materials with Elongación of 21.0 % | O | AA Standards, ASTM B209 | A50 | |
21.0 % Show Material materials with Elongación of 21.0 % | O | |||
22.0 % Show Material materials with Elongación of 22.0 % | O | AA Standards, ASTM B209 | A50 | |
25.0 % Show Material materials with Elongación of 25.0 % | O | AA Standards | A50 | |
25 % Show Material materials with Elongación of 25 % | O | |||
Límite elástico | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | AA Standards, ASTM B209, ASTM B210, ASTM B483 | RP02 |
40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | AA Standards | RP02 | |
40 MPa Show Material materials with Límite elástico of 40 MPa | O | RP02 | ||
41.0 MPa Show Material materials with Límite elástico of 41.0 MPa | O | |||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | O | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 | |
69 GPa Show Material materials with Módulo elástico of 69 GPa | O | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Resistencia a la tracción | 105.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 145.0 MPa | O | AA Standards, ASTM B209, ASTM B210 | |
105.0 MPa Show Material materials with Resistencia a la tracción of 105.0 MPa | O | AA Standards, ASTM B483 | ||
120.0 MPa Show Material materials with Resistencia a la tracción of 120.0 MPa | O | |||
125.0 MPa Show Material materials with Resistencia a la tracción of 125.0 MPa | O | AA Standards | ||
125 MPa Show Material materials with Resistencia a la tracción of 125 MPa | O | |||
140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | O | AA Standards, ASTM B316 | ||
Resistencia al cizallamiento | 76.0 MPa Show Material materials with Resistencia al cizallamiento of 76.0 MPa | O |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | |||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | O | |||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 | ||
Conductividad térmica | 200.0 W/(m·K) Show Material materials with Conductividad térmica of 200.0 W/(m·K) | O | |||
201 W/(m·K) Show Material materials with Conductividad térmica of 201 W/(m·K) | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 | |||
Temperatura de fusión | 630.0 - 655.0 °C Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 | ||
630.0 °C Show Material materials with Temperatura de fusión of 630.0 °C | O | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 30000000.0 S/m Show Material materials with Conductividad eléctrica of 30000000.0 S/m | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 | |
30200000 S/m Show Material materials with Conductividad eléctrica of 30200000 S/m | O | Typical/derived value | ||
Resistividad eléctrica | 3.33e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.33e-08 Ω·m | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 | |
Specific Electrical conductivity | 52.0 % IACS Show Material materials with Specific Electrical conductivity of 52.0 % IACS | O | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 97.0 - 99.5 % Show Material materials with Aluminio of 97.0 - 99.5 % | O | |
Cobre | 0.2 % Show Material materials with Cobre of 0.2 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 |
0.7 % Show Material materials with Hierro of 0.7 % | O | ||
Magnesio | 0.5 - 1.1 % Show Material materials with Magnesio of 0.5 - 1.1 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 |
Manganeso | 0.2 % Show Material materials with Manganeso of 0.2 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | O | |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B316, ASTM B483 |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12, H32), poor (H14, H34, H16, H18, H36, H38) | |
Workability | general (condition): good (O, H12, H32), acceptable (H14, H34), poor(H16, H18, H36, H38) |