General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H36 | ||
2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H36 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 95.0 MPa Show Material materials with Bending Fatigue Strength of 95.0 MPa | H36 | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Dureza Brinell | 58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | H36 | AA Standards | |
58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | H36 | 500 kg load, 10 mm ball | ||
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | H36 | AA Standards, ASTM B209 | A50 |
3.0 % Show Material materials with Elongación of 3.0 % | H36 | AA Standards, ASTM B209, ASTM B313 | A50 | |
4.0 % Show Material materials with Elongación of 4.0 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
4.7 % Show Material materials with Elongación of 4.7 % | H36 | |||
7.0 % Show Material materials with Elongación of 7.0 % | H36 | AA Standards | A50 | |
7 % Show Material materials with Elongación of 7 % | H36 | |||
Límite elástico | 150.0 MPa Show Material materials with Límite elástico of 150.0 MPa | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | RP02 |
180.0 MPa Show Material materials with Límite elástico of 180.0 MPa | H36 | AA Standards | RP02 | |
180 MPa Show Material materials with Límite elástico of 180 MPa | H36 | RP02 | ||
180.0 MPa Show Material materials with Límite elástico of 180.0 MPa | H36 | |||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H36 | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | |
69 GPa Show Material materials with Módulo elástico of 69 GPa | H36 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Resistencia a la fatiga | 97 MPa Show Material materials with Resistencia a la fatiga of 97 MPa | H36 | for 5x10⁸ cycles | |
Resistencia a la tracción | 185.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 185.0 - 230.0 MPa | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | H36 | AA Standards, ASTM B210, ASTM B483 | ||
205.0 MPa Show Material materials with Resistencia a la tracción of 205.0 MPa | H36 | AA Standards | ||
205 MPa Show Material materials with Resistencia a la tracción of 205 MPa | H36 | |||
210.0 MPa Show Material materials with Resistencia a la tracción of 210.0 MPa | H36 | |||
Resistencia al cizallamiento | 130.0 MPa Show Material materials with Resistencia al cizallamiento of 130.0 MPa | H36 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H36 | |||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H36 | |||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | ||
Conductividad térmica | 190.0 W/(m·K) Show Material materials with Conductividad térmica of 190.0 W/(m·K) | H36 | |||
193 W/(m·K) Show Material materials with Conductividad térmica of 193 W/(m·K) | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | |||
Temperatura de fusión | 625.0 - 650.0 °C Show Material materials with Temperatura de fusión of 625.0 - 650.0 °C | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | ||
630.0 °C Show Material materials with Temperatura de fusión of 630.0 °C | H36 | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 29000000.0 S/m Show Material materials with Conductividad eléctrica of 29000000.0 S/m | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Resistividad eléctrica | 3.45e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 Ω·m | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 96.3 - 98.9 % Show Material materials with Aluminio of 96.3 - 98.9 % | H36 | |
Cobre | 0.2 % Show Material materials with Cobre of 0.2 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
0.7 % Show Material materials with Hierro of 0.7 % | H36 | ||
Magnesio | 1.1 - 1.8 % Show Material materials with Magnesio of 1.1 - 1.8 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H36 | |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O), poor (H32, H34), sufficient (H36, H38) | |