General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547, BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet |
2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H32 | |||
2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H32 |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 115.0 MPa Show Material materials with Bending Fatigue Strength of 115.0 MPa | H32 | AA Standards | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | |||
Dureza Brinell | 60.0 [-] Show Material materials with Dureza Brinell of 60.0 [-] | H32 | AA Standards | ||
60.0 [-] Show Material materials with Dureza Brinell of 60.0 [-] | H32 | 500 kg load, 10 mm ball | |||
61.0 [-] Show Material materials with Dureza Brinell of 61.0 [-] | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | ||
Elongación | 4.0 % Show Material materials with Elongación of 4.0 % | H32 | AA Standards, ASTM B209 | A50 | |
5.0 % Show Material materials with Elongación of 5.0 % | H32 | AA Standards, ASTM B209, ASTM B313 | A50 | ||
7.0 % Show Material materials with Elongación of 7.0 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | ||
10.0 % Show Material materials with Elongación of 10.0 % | H32 | AA Standards, ASTM B209 | A100 | ||
11.0 % Show Material materials with Elongación of 11.0 % | H32 | AA Standards, ASTM B209, ASTM B547 | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | H32 | AA Standards | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | H32 | ||||
15 % Show Material materials with Elongación of 15 % | H32 | ||||
16.0 % Show Material materials with Elongación of 16.0 % | H32 | AA Standards | A100 | ||
Límite elástico | 130.0 MPa Show Material materials with Límite elástico of 130.0 MPa | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | RP02 |
160.0 MPa Show Material materials with Límite elástico of 160.0 MPa | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B483, ASTM B547 | RP02 | ||
180.0 MPa Show Material materials with Límite elástico of 180.0 MPa | H32 | ||||
195.0 MPa Show Material materials with Límite elástico of 195.0 MPa | H32 | AA Standards | RP02 | ||
195 MPa Show Material materials with Límite elástico of 195 MPa | H32 | RP02 | |||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H32 | |||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547, BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | |
70 GPa Show Material materials with Módulo elástico of 70 GPa | H32 | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | |||
Resistencia a la fatiga | 115 MPa Show Material materials with Resistencia a la fatiga of 115 MPa | H32 | for 5x10⁸ cycles | ||
Resistencia a la tracción | 210.0 - 260.0 MPa Show Material materials with Resistencia a la tracción of 210.0 - 260.0 MPa | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | |
215.0 - 265.0 MPa Show Material materials with Resistencia a la tracción of 215.0 - 265.0 MPa | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |||
215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | H32 | AA Standards, ASTM B210, ASTM B211, ASTM B234, ASTM B483 | |||
215.0 - 255.0 MPa Show Material materials with Resistencia a la tracción of 215.0 - 255.0 MPa | H32 | AA Standards, ASTM B316 | |||
230.0 MPa Show Material materials with Resistencia a la tracción of 230.0 MPa | H32 | AA Standards | |||
230 MPa Show Material materials with Resistencia a la tracción of 230 MPa | H32 | ||||
240.0 MPa Show Material materials with Resistencia a la tracción of 240.0 MPa | H32 | ||||
Resistencia al cizallamiento | 140.0 MPa Show Material materials with Resistencia al cizallamiento of 140.0 MPa | H32 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H32 | ||||
Coeficiente de dilatación térmica | 2.37e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.37e-05 1/K | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | ||
2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H32 | |||||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547 | |||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547 | |||
Conductividad térmica | 138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547 | |||
138.0 W/(m·K) Show Material materials with Conductividad térmica of 138.0 W/(m·K) | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | |||
140.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 W/(m·K) | H32 | |||||
Temperatura de fusión | 605.0 - 650.0 °C Show Material materials with Temperatura de fusión of 605.0 - 650.0 °C | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547 | |||
605.0 °C Show Material materials with Temperatura de fusión of 605.0 °C | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | |||
610.0 °C Show Material materials with Temperatura de fusión of 610.0 °C | H32 | |||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 20000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 S/m | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547 | |
Resistividad eléctrica | 4.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.95e-08 Ω·m | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet |
5e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 Ω·m | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminio | 95.8 - 97.7 % Show Material materials with Aluminio of 95.8 - 97.7 % | H32 | |||
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547, BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547 | ||
Hierro | 0.40 % Show Material materials with Hierro of 0.40 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547 | ||
0.4 % Show Material materials with Hierro of 0.4 % | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | ||
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547, BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547, BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H32 | BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | Total |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547, BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet | |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B316, ASTM B483, ASTM B547, BS EN 573-3, BS EN 485-2 | Sheet, Plate, Plate/Patterned Sheet |
Technological properties
Property | ||
---|---|---|
Application areas | Treadplate, Boilermaking, Containers, Nameplates, Road Signs, Architectural Paneling, Welded Tubes, Chemical Industry, Irrigation, Desalination units, Pressure Vessels, Rivets,Factory flooring, conveyors, indoor and outdoor walkways, steps, stairways, gantries, bridges, cranes, commercial vehicles | |
Brazing | general: limited brazing | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O, H32), sufficient (H34, H36, H38) | |
Soldering general | Not recommended | |
Welding | Gas: Good; Arc: Very Good; Resistance: Very Good | |
Workability | general (condition): good (O), acceptable (H32, H34), poor(H36, H38) |