Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 20.0 °C | 900 J/(kg·K) Show Material materials with Calor específico of 900 J/(kg·K) |
Coeficiente de dilatación térmica | 20.0 °C | 2.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4E-5 1/K |
Conductividad térmica | 20.0 °C | 140 W/(m·K) Show Material materials with Conductividad térmica of 140 W/(m·K) |
Temperatura de fusión | 610 °C Show Material materials with Temperatura de fusión of 610 °C |
General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 60 [-] Show Material materials with Dureza Brinell of 60 [-] |
Elongación | 20.0 °C | 12 % Show Material materials with Elongación of 12 % |
Elongación A50 | 20.0 °C | 4 - 12 % Show Material materials with Elongación A50 of 4 - 12 % |
Límite elástico | 20.0 °C | 180 MPa Show Material materials with Límite elástico of 180 MPa |
Límite elástico Rp 0,2 | 20.0 °C | 160 - 195 MPa Show Material materials with Límite elástico Rp 0,2 of 160 - 195 MPa |
Módulo elástico | 20.0 °C | 70 GPa Show Material materials with Módulo elástico of 70 GPa |
Resistencia a la tracción | 20.0 °C | 215 - 240 MPa Show Material materials with Resistencia a la tracción of 215 - 240 MPa |
Chemical properties
Property | Value |
---|---|
Aluminio | 95.8 - 97.7 % Show Material materials with Aluminio of 95.8 - 97.7 % |
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % |
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % |
Otro | 0.15 % Show Material materials with Otro of 0.15 % |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % |