General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.65 g/cm³ Show Material materials with Densidad of 2.65 g/cm³ | H32 | BS EN 573-3, BS EN 485-2 | Plate, Sheet |
2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H32 |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 160.0 MPa Show Material materials with Bending Fatigue Strength of 160.0 MPa | H32 | AA Standards | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | |||
Dureza Brinell | 89.0 [-] Show Material materials with Dureza Brinell of 89.0 [-] | H32 | BS EN 573-3, BS EN 485-2 | Plate, Sheet | |
Elongación | 8.5 % Show Material materials with Elongación of 8.5 % | H32 | |||
10.0 % Show Material materials with Elongación of 10.0 % | H32 | AA Standards, ASTM B209 | A100 | ||
10.0 % Show Material materials with Elongación of 10.0 % | H32 | AA Standards, ASTM B209 | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | H32 | AA Standards, ASTM B209 | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | H32 | AA Standards | A100 | ||
Límite elástico | 200.0 - 295.0 MPa Show Material materials with Límite elástico of 200.0 - 295.0 MPa | H32 | AA Standards, ASTM B209 | RP02 | |
215.0 - 295.0 MPa Show Material materials with Límite elástico of 215.0 - 295.0 MPa | H32 | AA Standards, ASTM B209 | RP02 | ||
230.0 MPa Show Material materials with Límite elástico of 230.0 MPa | H32 | AA Standards | RP02 | ||
240.0 MPa Show Material materials with Límite elástico of 240.0 MPa | H32 | ||||
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | |||
Módulo elástico | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | H32 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | |||
Resistencia a la tracción | 285.0 - 385.0 MPa Show Material materials with Resistencia a la tracción of 285.0 - 385.0 MPa | H32 | AA Standards, ASTM B209 | ||
305.0 - 385.0 MPa Show Material materials with Resistencia a la tracción of 305.0 - 385.0 MPa | H32 | AA Standards, ASTM B209 | |||
315.0 MPa Show Material materials with Resistencia a la tracción of 315.0 MPa | H32 | AA Standards | |||
330.0 MPa Show Material materials with Resistencia a la tracción of 330.0 MPa | H32 |
Aplicaciones térmicas
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H32 | |||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H32 | |||
Conductividad térmica | 120.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 W/(m·K) | H32 | |||
121.0 W/(m·K) Show Material materials with Conductividad térmica of 121.0 W/(m·K) | H32 | BS EN 573-3, BS EN 485-2 | Plate, Sheet | ||
Temperatura de fusión | 570.0 °C Show Material materials with Temperatura de fusión of 570.0 °C | H32 | BS EN 573-3, BS EN 485-2 | Plate, Sheet | |
580.0 °C Show Material materials with Temperatura de fusión of 580.0 °C | H32 | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Conductividad eléctrica | 18000000.0 - 31000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium | |||
Resistividad eléctrica | 5.8e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.8e-08 Ω·m | H32 | BS EN 573-3, BS EN 485-2 | Plate, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminio | 92.4 - 95.6 % Show Material materials with Aluminio of 92.4 - 95.6 % | H32 | |||
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H32 | AA Standards, ASTM B209, BS EN 573-3, BS EN 485-2 | Plate, Sheet | |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | H32 | AA Standards, ASTM B209, BS EN 573-3, BS EN 485-2 | Plate, Sheet | |
Hierro | 0.40 % Show Material materials with Hierro of 0.40 % | H32 | AA Standards, ASTM B209 | ||
0.4 % Show Material materials with Hierro of 0.4 % | H32 | BS EN 573-3, BS EN 485-2 | Plate, Sheet | ||
Magnesio | 4.0 - 4.9 % Show Material materials with Magnesio of 4.0 - 4.9 % | H32 | AA Standards, ASTM B209, BS EN 573-3, BS EN 485-2 | Plate, Sheet | |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | H32 | AA Standards, ASTM B209, BS EN 573-3, BS EN 485-2 | Plate, Sheet | |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H32 | BS EN 573-3, BS EN 485-2 | Plate, Sheet | Total |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H32 | AA Standards, ASTM B209, BS EN 573-3, BS EN 485-2 | Plate, Sheet | |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H32 | AA Standards, ASTM B209, BS EN 573-3, BS EN 485-2 | Plate, Sheet | |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H32 | AA Standards, ASTM B209, BS EN 573-3, BS EN 485-2 | Plate, Sheet |
Technological properties
Property | ||
---|---|---|
Application areas | Ship building, Rail cars, Vehicle bodies, Tip truck bodies, Mine skips and cages, Pressure vessels | |
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: kein Schadensfall im Betrieb und bei Labortests (O, H321, H116), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (H111), general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor | |
Soldering general | Poor | |
Welding | When welding 5083 to itself or another alloy from the same sub-group, the recommended filler metal is 5183. Other suitable fillers are 5356 and 5556. Gas: Average; Arc: Excellent; Resistance: Excellent | |