General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H34 | ||
2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H34 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Elongación | 4.0 % Show Material materials with Elongación of 4.0 % | H34 | AA Standards, ASTM B209 | A50 |
5.0 % Show Material materials with Elongación of 5.0 % | H34 | AA Standards, ASTM B209, ASTM B313 | A50 | |
6.0 % Show Material materials with Elongación of 6.0 % | H34 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
6.8 % Show Material materials with Elongación of 6.8 % | H34 | |||
9.0 % Show Material materials with Elongación of 9.0 % | H34 | AA Standards, ASTM B209 | A100 | |
10.0 % Show Material materials with Elongación of 10.0 % | H34 | AA Standards, ASTM B209, ASTM B547 | A50 | |
10 % Show Material materials with Elongación of 10 % | H34 | |||
Límite elástico | 235.0 MPa Show Material materials with Límite elástico of 235.0 MPa | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | RP02 |
255.0 MPa Show Material materials with Límite elástico of 255.0 MPa | H34 | AA Standards | RP02 | |
255 MPa Show Material materials with Límite elástico of 255 MPa | H34 | RP02 | ||
270.0 MPa Show Material materials with Límite elástico of 270.0 MPa | H34 | |||
Módulo de cizallamiento | 26.4 GPa Show Material materials with Módulo de cizallamiento of 26.4 GPa | H34 | ||
Módulo de compresión | 72.4 MPa Show Material materials with Módulo de compresión of 72.4 MPa | H34 | ||
Módulo elástico | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | |
71 GPa Show Material materials with Módulo elástico of 71 GPa | H34 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Resistencia a la tracción | 300.0 - 350.0 MPa Show Material materials with Resistencia a la tracción of 300.0 - 350.0 MPa | H34 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | H34 | AA Standards, ASTM B210 | ||
325.0 MPa Show Material materials with Resistencia a la tracción of 325.0 MPa | H34 | AA Standards | ||
325 MPa Show Material materials with Resistencia a la tracción of 325 MPa | H34 | |||
330.0 MPa Show Material materials with Resistencia a la tracción of 330.0 MPa | H34 | |||
Resistencia al cizallamiento | 185.0 MPa Show Material materials with Resistencia al cizallamiento of 185.0 MPa | H34 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H34 | |||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H34 | |||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | ||
Conductividad térmica | 126 W/(m·K) Show Material materials with Conductividad térmica of 126 W/(m·K) | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | ||
130.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 W/(m·K) | H34 | ||||
Temperatura de fusión | 585.0 - 640.0 °C Show Material materials with Temperatura de fusión of 585.0 - 640.0 °C | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | ||
590.0 °C Show Material materials with Temperatura de fusión of 590.0 °C | H34 | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 18000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 S/m | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Resistividad eléctrica | 5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.56e-08 Ω·m | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 93.0 - 96.3 % Show Material materials with Aluminio of 93.0 - 96.3 % | H34 | |
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Hierro | 0.50 % Show Material materials with Hierro of 0.50 % | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
0.5 % Show Material materials with Hierro of 0.5 % | H34 | ||
Magnesio | 3.5 - 4.5 % Show Material materials with Magnesio of 3.5 - 4.5 % | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Manganeso | 0.2 - 0.7 % Show Material materials with Manganeso of 0.2 - 0.7 % | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H34 | |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H34 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests (O, H32, H116, H111), no damage during operation, limited damage during laboratory tests (H34, H36, H38), general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O, H32, H116, H111), sufficient (H34, H36, H38) | |
Workability | general (condition): good (O), acceptable (H32, H116, H111), poor(H36, H38) |