General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H32 | ||
2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H32 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | H32 | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Dureza Brinell | 67.0 [-] Show Material materials with Dureza Brinell of 67.0 [-] | H32 | AA Standards | |
67.0 [-] Show Material materials with Dureza Brinell of 67.0 [-] | H32 | 500 kg load, 10 mm ball | ||
Elongación | 5.0 % Show Material materials with Elongación of 5.0 % | H32 | AA Standards, ASTM B209 | A50 |
6.0 % Show Material materials with Elongación of 6.0 % | H32 | AA Standards, ASTM B209, ASTM B313 | A50 | |
8.0 % Show Material materials with Elongación of 8.0 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
10.0 % Show Material materials with Elongación of 10.0 % | H32 | AA Standards, ASTM B209 | A100 | |
12.0 % Show Material materials with Elongación of 12.0 % | H32 | AA Standards, ASTM B209, ASTM B547 | A50 | |
12.0 % Show Material materials with Elongación of 12.0 % | H32 | |||
15.0 % Show Material materials with Elongación of 15.0 % | H32 | AA Standards | A50 | |
15 % Show Material materials with Elongación of 15 % | H32 | |||
Límite elástico | 180.0 MPa Show Material materials with Límite elástico of 180.0 MPa | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | RP02 |
200.0 MPa Show Material materials with Límite elástico of 200.0 MPa | H32 | |||
205.0 MPa Show Material materials with Límite elástico of 205.0 MPa | H32 | AA Standards | RP02 | |
205 MPa Show Material materials with Límite elástico of 205 MPa | H32 | RP02 | ||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H32 | ||
Módulo de compresión | 70.7 MPa Show Material materials with Módulo de compresión of 70.7 MPa | H32 | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 | |
70 GPa Show Material materials with Módulo elástico of 70 GPa | H32 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Resistencia a la fatiga | 124 MPa Show Material materials with Resistencia a la fatiga of 124 MPa | H32 | for 5x10⁸ cycles | |
Resistencia a la tracción | 250.0 - 300.0 MPa Show Material materials with Resistencia a la tracción of 250.0 - 300.0 MPa | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | H32 | AA Standards, ASTM B211 | ||
270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H32 | AA Standards | ||
270 MPa Show Material materials with Resistencia a la tracción of 270 MPa | H32 | |||
Resistencia al cizallamiento | 152.0 MPa Show Material materials with Resistencia al cizallamiento of 152.0 MPa | H32 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H32 | |||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H32 | |||
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 | ||
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 | ||
Conductividad térmica | 126 W/(m·K) Show Material materials with Conductividad térmica of 126 W/(m·K) | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 | ||
130.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 W/(m·K) | H32 | ||||
Temperatura de fusión | 590.0 - 645.0 °C Show Material materials with Temperatura de fusión of 590.0 - 645.0 °C | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 | ||
590.0 °C Show Material materials with Temperatura de fusión of 590.0 °C | H32 | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 19000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 S/m | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Resistividad eléctrica | 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.26e-08 Ω·m | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 94.4 - 96.8 % Show Material materials with Aluminio of 94.4 - 96.8 % | H32 | |
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Hierro | 0.40 % Show Material materials with Hierro of 0.40 % | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
0.4 % Show Material materials with Hierro of 0.4 % | H32 | ||
Magnesio | 3.1 - 3.9 % Show Material materials with Magnesio of 3.1 - 3.9 % | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H32 | |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H32 | AA Standards, ASTM B209, ASTM B211, ASTM B313, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O, H32), sufficient (H34, H36, H38) | |
Workability | general (condition): good (O), acceptable (H32, H34), poor(H36, H38) |