General
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Dureza Brinell | 95.0 [-] Show Material materials with Dureza Brinell of 95.0 [-] | T5 | 500 kg load, 10 mm ball | |
Elongación | 8.0 % Show Material materials with Elongación of 8.0 % | T5 | AA Standards, ASTM B221 | A50 |
9.0 % Show Material materials with Elongación of 9.0 % | T5 | AA Standards, ASTM B221 | A100 | |
9.6 % Show Material materials with Elongación of 9.6 % | T5 | |||
10.0 % Show Material materials with Elongación of 10.0 % | T5 | AA Standards, ASTM B221 | A50 | |
Límite elástico | 240.0 MPa Show Material materials with Límite elástico of 240.0 MPa | T5 | AA Standards, ASTM B221 | RP02 |
270.0 MPa Show Material materials with Límite elástico of 270.0 MPa | T5 | |||
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Módulo de compresión | 69.6 MPa Show Material materials with Módulo de compresión of 69.6 MPa | T5 | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | T5 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Resistencia a la fatiga | 97 MPa Show Material materials with Resistencia a la fatiga of 97 MPa | T5 | Min., for 5x10⁸ cycles | |
Resistencia a la tracción | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | T5 | AA Standards, ASTM B221 | |
290.0 MPa Show Material materials with Resistencia a la tracción of 290.0 MPa | T5 | |||
Resistencia al cizallamiento | 205.0 MPa Show Material materials with Resistencia al cizallamiento of 205.0 MPa | T5 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | T5 | ||
Coeficiente de dilatación térmica | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T5 | ||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T5 | AA Standards, ASTM B221 | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T5 | AA Standards, ASTM B221 | |
Conductividad térmica | 180.0 - 188.0 W/(m·K) Show Material materials with Conductividad térmica of 180.0 - 188.0 W/(m·K) | T5 | AA Standards, ASTM B221 | |
180.0 W/(m·K) Show Material materials with Conductividad térmica of 180.0 W/(m·K) | T5 | |||
Temperatura de fusión | 605.0 - 655.0 °C Show Material materials with Temperatura de fusión of 605.0 - 655.0 °C | T5 | AA Standards, ASTM B221 | |
610.0 °C Show Material materials with Temperatura de fusión of 610.0 °C | T5 |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 27000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 27000000.0 - 28000000.0 S/m | T5 | AA Standards, ASTM B221 | |
28000000 S/m Show Material materials with Conductividad eléctrica of 28000000 S/m | T5 | Typical/derived value | ||
Resistividad eléctrica | 3.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.5e-08 Ω·m | T5 | Typical value | |
3.57e-08 - 3.7e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.57e-08 - 3.7e-08 Ω·m | T5 | AA Standards, ASTM B221 | ||
Specific Electrical conductivity | 49.0 % IACS Show Material materials with Specific Electrical conductivity of 49.0 % IACS | T5 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 97.5 - 99.0 % Show Material materials with Aluminio of 97.5 - 99.0 % | T5 | |
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | T5 | AA Standards, ASTM B221 |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | T5 | AA Standards, ASTM B221 |
Hierro | 0.35 % Show Material materials with Hierro of 0.35 % | T5 | AA Standards, ASTM B221 |
0.35 % Show Material materials with Hierro of 0.35 % | T5 | ||
Magnesio | 0.4 - 0.6 % Show Material materials with Magnesio of 0.4 - 0.6 % | T5 | AA Standards, ASTM B221 |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | T5 | AA Standards, ASTM B221 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T5 | |
Silicona | 0.6 - 0.9 % Show Material materials with Silicona of 0.6 - 0.9 % | T5 | AA Standards, ASTM B221 |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | T5 | AA Standards, ASTM B221 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | T5 | AA Standards, ASTM B221 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Workability | Excellent workability. |