General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | O | ||
2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | O | EN 573-3, EN 485-2 | Sheet |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |||
Dureza Brinell | 20.0 [-] Show Material materials with Dureza Brinell of 20.0 [-] | O | EN 573-3, EN 485-2 | Sheet | |
Elongación | 39.0 % Show Material materials with Elongación of 39.0 % | O | |||
Límite elástico | 20.0 MPa Show Material materials with Límite elástico of 20.0 MPa | O | EN 573-3, EN 485-2 | Sheet | RP02 |
26.0 MPa Show Material materials with Límite elástico of 26.0 MPa | O | ||||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | |||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | |||
71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | O | EN 573-3, EN 485-2 | Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |||
Resistencia a la tracción | 65.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 65.0 - 95.0 MPa | O | EN 573-3, EN 485-2 | Sheet | |
77.0 MPa Show Material materials with Resistencia a la tracción of 77.0 MPa | O |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | ||||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | O | EN 573-3, EN 485-2 | Sheet | ||
Conductividad térmica | 222.0 W/(m·K) Show Material materials with Conductividad térmica of 222.0 W/(m·K) | O | EN 573-3, EN 485-2 | Sheet | ||
230.0 W/(m·K) Show Material materials with Conductividad térmica of 230.0 W/(m·K) | O | |||||
20 °C | 231 W/(m·K) Show Material materials with Conductividad térmica of 231 W/(m·K) | O | unstated value | |||
Temperatura de fusión | 650.0 °C Show Material materials with Temperatura de fusión of 650.0 °C | O | EN 573-3, EN 485-2 | Sheet |
Eléctrico
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Conductividad eléctrica | 33000000.0 - 38000000.0 S/m Show Material materials with Conductividad eléctrica of 33000000.0 - 38000000.0 S/m | Typical for Wrought 1000 Series Aluminium | |||
Resistividad eléctrica | 2.82e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.82e-08 Ω·m | O | EN 573-3, EN 485-2 | Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminio | 99.5 - 100.0 % Show Material materials with Aluminio of 99.5 - 100.0 % | O | |||
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | O | EN 573-3, EN 485-2 | Sheet | |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | O | EN 573-3, EN 485-2 | Sheet | |
Magnesio | 0.05 % Show Material materials with Magnesio of 0.05 % | O | EN 573-3, EN 485-2 | Sheet | |
Manganeso | 0.05 % Show Material materials with Manganeso of 0.05 % | O | EN 573-3, EN 485-2 | Sheet | |
Otro | 0.03 % Show Material materials with Otro of 0.03 % | O | EN 573-3, EN 485-2 | Sheet | Each |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | O | EN 573-3, EN 485-2 | Sheet | |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | O | |||
0.05 % Show Material materials with Titanio of 0.05 % | O | EN 573-3, EN 485-2 | Sheet | ||
Vanadio | 0.05 % Show Material materials with Vanadio of 0.05 % | O | |||
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | O | |||
0.07 % Show Material materials with Zinc of 0.07 % | O | EN 573-3, EN 485-2 | Sheet |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical process plant equipment, Food industry containers, Pyrotechnic powder, Architectural flashings, Lamp reflectors, Cable sheathing | |
Brazing | Excellent | |
General machinability | Poor | |
Soldering general | Excellent | |
Welding | When welding 1050 to itself or an alloy from the same subgroup the recommended filler wire is 1100. For welding to alloys 5083 and 5086 or alloys from the 7XXX series, the recommend wire is 5356. For other alloys use 4043 filler wire. Gas: Excellent; Arc: Excellent; Resistance: Excellent | |
Workability | Cold: Excellent |