General
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 60.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 MPa | O | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | O | ||
Dureza Brinell | 30.0 [-] Show Material materials with Dureza Brinell of 30.0 [-] | O | AA Standards | |
30.0 [-] Show Material materials with Dureza Brinell of 30.0 [-] | O | 500 kg load, 10 mm ball | ||
Elongación | 10.0 % Show Material materials with Elongación of 10.0 % | O | AA Standards, ASTM B209 | A50 |
12.0 % Show Material materials with Elongación of 12.0 % | O | AA Standards, ASTM B209 | A50 | |
13.0 % Show Material materials with Elongación of 13.0 % | O | AA Standards, ASTM B210, ASTM B483 | A100 | |
14.0 % Show Material materials with Elongación of 14.0 % | O | AA Standards, ASTM B209 | A50 | |
14.0 % Show Material materials with Elongación of 14.0 % | O | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B345 | A100 | |
15.0 % Show Material materials with Elongación of 15.0 % | O | AA Standards, ASTM B210, ASTM B483 | A50 | |
16.0 % Show Material materials with Elongación of 16.0 % | O | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B313, ASTM B345 | A50 | |
16.0 % Show Material materials with Elongación of 16.0 % | O | AA Standards, ASTM B209, ASTM B211 | A100 | |
17.0 % Show Material materials with Elongación of 17.0 % | O | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | AA Standards, ASTM B209, ASTM B211 | A50 | |
20.0 % Show Material materials with Elongación of 20.0 % | O | |||
25.0 % Show Material materials with Elongación of 25.0 % | O | AA Standards | A50 | |
27.0 % Show Material materials with Elongación of 27.0 % | O | AA Standards | A100 | |
27.5 % Show Material materials with Elongación of 27.5 % | O | |||
Límite elástico | 55.0 MPa Show Material materials with Límite elástico of 55.0 MPa | O | AA Standards | RP02 |
55 MPa Show Material materials with Límite elástico of 55 MPa | O | RP02 | ||
75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | O | |||
85.0 MPa Show Material materials with Límite elástico of 85.0 MPa | O | AA Standards, ASTM B209 | RP02 | |
95.0 MPa Show Material materials with Límite elástico of 95.0 MPa | O | AA Standards, ASTM B210, ASTM B483 | RP02 | |
103.0 MPa Show Material materials with Límite elástico of 103.0 MPa | O | |||
110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | O | AA Standards, ASTM B221, ASTM B241 | RP02 | |
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Módulo de compresión | 69.7 MPa Show Material materials with Módulo de compresión of 69.7 MPa | O | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 | |
69 GPa Show Material materials with Módulo elástico of 69 GPa | O | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Resistencia a la tracción | 125.0 MPa Show Material materials with Resistencia a la tracción of 125.0 MPa | O | AA Standards | |
125 MPa Show Material materials with Resistencia a la tracción of 125 MPa | O | |||
130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | O | |||
150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | O | AA Standards, ASTM B209, ASTM B210, ASTM B221, ASTM B241, ASTM B313, ASTM B345, ASTM B483 | ||
155.0 MPa Show Material materials with Resistencia a la tracción of 155.0 MPa | O | AA Standards, ASTM B211, ASTM B316 | ||
228.0 MPa Show Material materials with Resistencia a la tracción of 228.0 MPa | O | |||
Resistencia al cizallamiento | 83.0 MPa Show Material materials with Resistencia al cizallamiento of 83.0 MPa | O |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 896.0 J/(kg·K) Show Material materials with Calor específico of 896.0 J/(kg·K) | O | ||
900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | |||
Coeficiente de dilatación térmica | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | ||
2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | O | |||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 | |
Conductividad térmica | 155.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 155.0 - 180.0 W/(m·K) | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 | |
170.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 W/(m·K) | O | |||
180.0 W/(m·K) Show Material materials with Conductividad térmica of 180.0 W/(m·K) | O | |||
Temperatura de fusión | 580.0 - 650.0 °C Show Material materials with Temperatura de fusión of 580.0 - 650.0 °C | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 | |
580.0 °C Show Material materials with Temperatura de fusión of 580.0 °C | O |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 27000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 27000000.0 S/m | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 | |
27000000 S/m Show Material materials with Conductividad eléctrica of 27000000 S/m | O | Typical value | ||
Resistividad eléctrica | 3.7e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.7e-08 - 4.35e-08 Ω·m | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 | |
3.7e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.7e-08 Ω·m | O | Typical value | ||
Specific Electrical conductivity | 47.0 % IACS Show Material materials with Specific Electrical conductivity of 47.0 % IACS | O | Typical/Derived value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 95.9 - 98.6 % Show Material materials with Aluminio of 95.9 - 98.6 % | O | |
Cobre | 0.15 - 0.4 % Show Material materials with Cobre of 0.15 - 0.4 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 |
Cromo | 0.04 - 0.35 % Show Material materials with Cromo of 0.04 - 0.35 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 |
0.7 % Show Material materials with Hierro of 0.7 % | O | ||
Magnesio | 0.8 - 1.2 % Show Material materials with Magnesio of 0.8 - 1.2 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 |
Manganeso | 0.15 % Show Material materials with Manganeso of 0.15 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | O | |
Silicona | 0.4 - 0.8 % Show Material materials with Silicona of 0.4 - 0.8 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B313, ASTM B316, ASTM B345, ASTM B483 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests (O, T6, T651, T652, T6510, T6511), no damage during operation, limited damage during laboratory tests (T4, T451, T4510, T4511), general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O), sufficient (T4, T451, T4510, T4511, T6, T651, T652, T6510, T6511) | |
Workability | general (condition): good (O), acceptable (T4, T451, T4510, T4511), poor(T6, T651, T652, T6510, T6511) |