General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |||
Dureza Brinell | 84.0 - 91.0 [-] Show Material materials with Dureza Brinell of 84.0 - 91.0 [-] | T6 | BS EN 573-3, BS EN 485-2 | Plate | |
94.0 [-] Show Material materials with Dureza Brinell of 94.0 [-] | T6 | BS EN 573-3, BS EN 485-2 | Sheet | ||
95.0 [-] Show Material materials with Dureza Brinell of 95.0 [-] | T6 | BS EN 573-3, BS EN 755-2 | Bar, Tube | ||
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2 | Bar, Tube | A50 |
6.0 - 10.0 % Show Material materials with Elongación of 6.0 - 10.0 % | T6 | BS EN 573-3, BS EN 755-2 | Bar, Tube | ||
8.0 % Show Material materials with Elongación of 8.0 % | T6 | AA Standards, ASTM B221 | A100 | ||
8.5 % Show Material materials with Elongación of 8.5 % | T6 | ||||
9.0 % Show Material materials with Elongación of 9.0 % | T6 | BS EN 573-3, BS EN 485-2 | Plate | A50 | |
Límite elástico | 200.0 - 260.0 MPa Show Material materials with Límite elástico of 200.0 - 260.0 MPa | T6 | BS EN 573-3, BS EN 755-2 | Bar, Tube | RP02 |
240.0 - 255.0 MPa Show Material materials with Límite elástico of 240.0 - 255.0 MPa | T6 | BS EN 573-3, BS EN 485-2 | Plate | RP02 | |
260.0 MPa Show Material materials with Límite elástico of 260.0 MPa | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 485-2 | Sheet | RP02 | |
280.0 MPa Show Material materials with Límite elástico of 280.0 MPa | T6 | ||||
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | |||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T6 | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |||
Resistencia a la tracción | 270.0 - 310.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 310.0 MPa | T6 | BS EN 573-3, BS EN 755-2 | Bar, Tube | |
275.0 - 300.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 300.0 MPa | T6 | BS EN 573-3, BS EN 485-2 | Plate | ||
310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 485-2 | Sheet | ||
330.0 MPa Show Material materials with Resistencia a la tracción of 330.0 MPa | T6 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 890.0 J/(kg·K) Show Material materials with Calor específico of 890.0 J/(kg·K) | T6 | ||||
Coeficiente de dilatación térmica | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T6 | ||||
2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |||
100 °C | 0.000022 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000022 1/K | T6 | unstated value for 20-100°C | |||
Conductividad térmica | 170.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 W/(m·K) | T6 | ||||
180.0 W/(m·K) Show Material materials with Conductividad térmica of 180.0 W/(m·K) | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |||
Temperatura de fusión | 555.0 °C Show Material materials with Temperatura de fusión of 555.0 °C | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | ||
580.0 °C Show Material materials with Temperatura de fusión of 580.0 °C | T6 |
Eléctrico
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Conductividad eléctrica | 21000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium | |||
Resistividad eléctrica | 3.8e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.8e-08 Ω·m | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminio | 95.2 - 98.3 % Show Material materials with Aluminio of 95.2 - 98.3 % | T6 | |||
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Hierro | 0.50 % Show Material materials with Hierro of 0.50 % | T6 | AA Standards, ASTM B221 | ||
0.5 % Show Material materials with Hierro of 0.5 % | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | ||
Magnesio | 0.6 - 1.2 % Show Material materials with Magnesio of 0.6 - 1.2 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | Total |
Silicona | 0.7 - 1.3 % Show Material materials with Silicona of 0.7 - 1.3 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet |
Technological properties
Property | ||
---|---|---|
Application areas | Highly stressed applications, Trusses, Bridges, Cranes, Transport applications, Ore skips, Beer barrels, Milk churns | |
Brazing | Good | |
General machinability | Good | |
Soldering general | Good | |
Welding | 6082 has very good weldability but strength is lowered in the weld zone. When welded to itself, alloy 4043 wire is recommended. If welding 6082 to 7005, then the wire used should be alloy 5356. Gas: Good; Arc: Good; Resistance: Good | |
Workability | Cold: Good |