General
Property | Value | Condition |
---|---|---|
Densidad | 2.81 g/cm³ Show Material materials with Densidad of 2.81 g/cm³ | T7352 |
3.1 g/cm³ Show Material materials with Densidad of 3.1 g/cm³ | T7352 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | T7352 | AA Standards, ASTM B247 | A100 |
2.0 % Show Material materials with Elongación of 2.0 % | T7352 | AA Standards, ASTM B247 | A50 | |
2.0 % Show Material materials with Elongación of 2.0 % | T7352 | AA Standards, ASTM B247 | A100 | |
3.0 % Show Material materials with Elongación of 3.0 % | T7352 | AA Standards, ASTM B247 | A50 | |
3.0 % Show Material materials with Elongación of 3.0 % | T7352 | AA Standards, ASTM B247 | A100 | |
3.2 % Show Material materials with Elongación of 3.2 % | T7352 | |||
5.0 % Show Material materials with Elongación of 5.0 % | T7352 | AA Standards, ASTM B247 | A100 | |
6.0 % Show Material materials with Elongación of 6.0 % | T7352 | AA Standards, ASTM B247 | A100 | |
7.0 % Show Material materials with Elongación of 7.0 % | T7352 | AA Standards, ASTM B247 | A50 | |
Límite elástico | 305.0 MPa Show Material materials with Límite elástico of 305.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 |
315.0 MPa Show Material materials with Límite elástico of 315.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
330.0 MPa Show Material materials with Límite elástico of 330.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
340.0 MPa Show Material materials with Límite elástico of 340.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
345.0 MPa Show Material materials with Límite elástico of 345.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
350.0 MPa Show Material materials with Límite elástico of 350.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
360.0 MPa Show Material materials with Límite elástico of 360.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
365.0 MPa Show Material materials with Límite elástico of 365.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
370.0 MPa Show Material materials with Límite elástico of 370.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
385.0 MPa Show Material materials with Límite elástico of 385.0 MPa | T7352 | AA Standards, ASTM B247 | RP02 | |
390.0 MPa Show Material materials with Límite elástico of 390.0 MPa | T7352 | |||
Módulo de cizallamiento | 26.4 - 27.1 GPa Show Material materials with Módulo de cizallamiento of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||
Módulo elástico | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T7352 | ||
Plane-Strain Fracture Toughnes | 28 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28 MPa·√m | T7352 | For forging in T-L direction | |
30 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30 MPa·√m | T7352 | For forging in T-L direction | ||
Resistencia a la tracción | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T7352 | AA Standards, ASTM B247 | |
400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T7352 | AA Standards, ASTM B247 | ||
405.0 MPa Show Material materials with Resistencia a la tracción of 405.0 MPa | T7352 | AA Standards, ASTM B247 | ||
415.0 MPa Show Material materials with Resistencia a la tracción of 415.0 MPa | T7352 | AA Standards, ASTM B247 | ||
420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T7352 | AA Standards, ASTM B247 | ||
425.0 MPa Show Material materials with Resistencia a la tracción of 425.0 MPa | T7352 | AA Standards, ASTM B247 | ||
435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T7352 | AA Standards, ASTM B247 | ||
440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T7352 | AA Standards, ASTM B247 | ||
455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T7352 | AA Standards, ASTM B247 | ||
470.0 MPa Show Material materials with Resistencia a la tracción of 470.0 MPa | T7352 |
Aplicaciones térmicas
Property | Value | Condition |
---|---|---|
Calor específico | 910.0 J/(kg·K) Show Material materials with Calor específico of 910.0 J/(kg·K) | T7352 |
Coeficiente de dilatación térmica | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T7352 |
Conductividad térmica | 130.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 W/(m·K) | T7352 |
Temperatura de fusión | 480.0 °C Show Material materials with Temperatura de fusión of 480.0 °C | T7352 |
Eléctrico
Property | Value | Condition | Comment |
---|---|---|---|
Conductividad eléctrica | 23000000 S/m Show Material materials with Conductividad eléctrica of 23000000 S/m | T7352 | Typical/derived value |
Resistividad eléctrica | 4.3099999999999996e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.3099999999999996e-08 Ω·m | T7352 | Typical value |
Specific Electrical conductivity | 40.0 % IACS Show Material materials with Specific Electrical conductivity of 40.0 % IACS | T7352 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 86.9 - 91.4 % Show Material materials with Aluminio of 86.9 - 91.4 % | T7352 | |
Circonio | 0.25 % Show Material materials with Circonio of 0.25 % | T7352 | |
Cobre | 1.2 - 2.0 % Show Material materials with Cobre of 1.2 - 2.0 % | T7352 | AA Standards, ASTM B247 |
Cromo | 0.18 - 0.28 % Show Material materials with Cromo of 0.18 - 0.28 % | T7352 | AA Standards, ASTM B247 |
Hierro | 0.50 % Show Material materials with Hierro of 0.50 % | T7352 | AA Standards, ASTM B247 |
0.5 % Show Material materials with Hierro of 0.5 % | T7352 | ||
Magnesio | 2.1 - 2.9 % Show Material materials with Magnesio of 2.1 - 2.9 % | T7352 | AA Standards, ASTM B247 |
Manganeso | 0.3 % Show Material materials with Manganeso of 0.3 % | T7352 | AA Standards, ASTM B247 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T7352 | |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | T7352 | AA Standards, ASTM B247 |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | T7352 | AA Standards, ASTM B247 |
Zinc | 5.1 - 6.1 % Show Material materials with Zinc of 5.1 - 6.1 % | T7352 | AA Standards, ASTM B247 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O), good to acceptable | |
Workability | general (condition): not suitable |