General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | O | |
2.705 g/cm³ Show Material materials with Densidad of 2.705 g/cm³ | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 20.0 MPa Show Material materials with Bending Fatigue Strength of 20.0 MPa | O | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||
Dureza Brinell | 19.0 [-] Show Material materials with Dureza Brinell of 19.0 [-] | O | AA Standards | |
23.0 [-] Show Material materials with Dureza Brinell of 23.0 [-] | O | 500 kg load, 10 mm ball | ||
Elongación | 15.0 % Show Material materials with Elongación of 15.0 % | O | AA Standards, ASTM B209 | A50 |
18.0 % Show Material materials with Elongación of 18.0 % | O | AA Standards, ASTM B209 | A50 | |
22.0 % Show Material materials with Elongación of 22.0 % | O | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B345 | A100 | |
23.0 % Show Material materials with Elongación of 23.0 % | O | AA Standards, ASTM B209 | A50 | |
25.0 % Show Material materials with Elongación of 25.0 % | O | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B345 | A50 | |
31.0 % Show Material materials with Elongación of 31.0 % | O | |||
43.0 % Show Material materials with Elongación of 43.0 % | O | AA Standards | A50 | |
43 % Show Material materials with Elongación of 43 % | O | |||
Límite elástico | 15.0 MPa Show Material materials with Límite elástico of 15.0 MPa | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | RP02 |
21.0 MPa Show Material materials with Límite elástico of 21.0 MPa | O | |||
30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | O | AA Standards | RP02 | |
30 MPa Show Material materials with Límite elástico of 30 MPa | O | RP02 | ||
Módulo de cizallamiento | 25.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 GPa | O | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
69 GPa Show Material materials with Módulo elástico of 69 GPa | O | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||
Resistencia a la fatiga | 21 MPa Show Material materials with Resistencia a la fatiga of 21 MPa | O | for 5x10⁸ cycles | |
Resistencia a la tracción | 55.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 55.0 - 95.0 MPa | O | AA Standards, ASTM B209 | |
55.0 MPa Show Material materials with Resistencia a la tracción of 55.0 MPa | O | AA Standards, ASTM B211 | ||
60.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 60.0 - 95.0 MPa | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
70.0 MPa Show Material materials with Resistencia a la tracción of 70.0 MPa | O | AA Standards | ||
70 MPa Show Material materials with Resistencia a la tracción of 70 MPa | O | |||
72.0 MPa Show Material materials with Resistencia a la tracción of 72.0 MPa | O | |||
Resistencia al cizallamiento | 50.0 MPa Show Material materials with Resistencia al cizallamiento of 50.0 MPa | O |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | |||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | O | |||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
Conductividad térmica | 230.0 - 234.0 W/(m·K) Show Material materials with Conductividad térmica of 230.0 - 234.0 W/(m·K) | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
230.0 W/(m·K) Show Material materials with Conductividad térmica of 230.0 W/(m·K) | O | ||||
25 °C | 234 W/(m·K) Show Material materials with Conductividad térmica of 234 W/(m·K) | O | unstated value | ||
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
650.0 °C Show Material materials with Temperatura de fusión of 650.0 °C | O |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 35000000.0 - 36000000.0 S/m Show Material materials with Conductividad eléctrica of 35000000.0 - 36000000.0 S/m | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
36000000 S/m Show Material materials with Conductividad eléctrica of 36000000 S/m | O | Typical/derived value | ||
Resistividad eléctrica | 2.78e-08 - 2.86e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.78e-08 - 2.86e-08 Ω·m | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
Specific Electrical conductivity | 62.0 % IACS Show Material materials with Specific Electrical conductivity of 62.0 % IACS | O | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 99.6 % Show Material materials with Aluminio of 99.6 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
99.6 - 100.0 % Show Material materials with Aluminio of 99.6 - 100.0 % | O | ||
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Hierro | 0.35 % Show Material materials with Hierro of 0.35 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
0.35 % Show Material materials with Hierro of 0.35 % | O | ||
Magnesio | 0.03 % Show Material materials with Magnesio of 0.03 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Manganeso | 0.03 % Show Material materials with Manganeso of 0.03 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Vanadio | 0.05 % Show Material materials with Vanadio of 0.05 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H16, H18) | |
Workability | general (condition): good (O, H12, H14), acceptable (H16, H18) |