General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 |
2.8 g/cm³ Show Material materials with Densidad of 2.8 g/cm³ | H112 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||
Elongación | 9.0 % Show Material materials with Elongación of 9.0 % | H112 | AA Standards, ASTM B209 | A50 |
12.0 % Show Material materials with Elongación of 12.0 % | H112 | AA Standards, ASTM B209 | A100 | |
16.0 % Show Material materials with Elongación of 16.0 % | H112 | AA Standards, ASTM B247 | A100 | |
18.0 % Show Material materials with Elongación of 18.0 % | H112 | AA Standards, ASTM B209 | A100 | |
18.0 % Show Material materials with Elongación of 18.0 % | H112 | AA Standards, ASTM B247 | A50 | |
20.0 % Show Material materials with Elongación of 20.0 % | H112 | AA Standards, ASTM B211 | A50 | |
21.0 % Show Material materials with Elongación of 21.0 % | H112 | |||
22.0 % Show Material materials with Elongación of 22.0 % | H112 | AA Standards, ASTM B241 | A100 | |
25.0 % Show Material materials with Elongación of 25.0 % | H112 | AA Standards, ASTM B241 | A50 | |
Límite elástico | 20.0 MPa Show Material materials with Límite elástico of 20.0 MPa | H112 | AA Standards, ASTM B211, ASTM B241 | RP02 |
30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | H112 | AA Standards, ASTM B209, ASTM B247 | RP02 | |
36.0 MPa Show Material materials with Límite elástico of 36.0 MPa | H112 | |||
40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | H112 | AA Standards, ASTM B209 | RP02 | |
50.0 MPa Show Material materials with Límite elástico of 50.0 MPa | H112 | AA Standards, ASTM B209 | RP02 | |
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||
Resistencia a la tracción | 75.0 MPa Show Material materials with Resistencia a la tracción of 75.0 MPa | H112 | AA Standards, ASTM B211, ASTM B241, ASTM B247 | |
80.0 MPa Show Material materials with Resistencia a la tracción of 80.0 MPa | H112 | AA Standards, ASTM B209 | ||
85.0 MPa Show Material materials with Resistencia a la tracción of 85.0 MPa | H112 | AA Standards, ASTM B209 | ||
90.0 MPa Show Material materials with Resistencia a la tracción of 90.0 MPa | H112 | AA Standards, ASTM B209 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H112 | ||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H112 | ||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 | |
Conductividad térmica | 218.0 - 222.0 W/(m·K) Show Material materials with Conductividad térmica of 218.0 - 222.0 W/(m·K) | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 | |
220.0 W/(m·K) Show Material materials with Conductividad térmica of 220.0 W/(m·K) | H112 | |||
Temperatura de fusión | 640.0 - 655.0 °C Show Material materials with Temperatura de fusión of 640.0 - 655.0 °C | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 | |
640.0 °C Show Material materials with Temperatura de fusión of 640.0 °C | H112 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 33000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 33000000.0 - 34000000.0 S/m | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 |
Resistividad eléctrica | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.94e-08 - 3.03e-08 Ω·m | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 99.0 % Show Material materials with Aluminio of 99.0 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 |
99.0 - 100.0 % Show Material materials with Aluminio of 99.0 - 100.0 % | H112 | ||
Cobre | 0.05 - 0.2 % Show Material materials with Cobre of 0.05 - 0.2 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 |
Hierro | 1.0 % Show Material materials with Hierro of 1.0 % | H112 | |
Manganeso | 0.05 % Show Material materials with Manganeso of 0.05 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H112 | |
Silicona | 1.0 % Show Material materials with Silicona of 1.0 % | H112 | |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B241, ASTM B247 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H16, H18) | |
Workability | general (condition): good (O, H12, H14), acceptable (H16), poor(H18) |