General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H19 | |
2.705 g/cm³ Show Material materials with Densidad of 2.705 g/cm³ | H19 | AA Standards |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 50.0 MPa Show Material materials with Bending Fatigue Strength of 50.0 MPa | H19 | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||
Elongación | 1.4 % Show Material materials with Elongación of 1.4 % | H19 | ||
Límite elástico | 165.0 MPa Show Material materials with Límite elástico of 165.0 MPa | H19 | AA Standards | RP02 |
170.0 MPa Show Material materials with Límite elástico of 170.0 MPa | H19 | |||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H19 | AA Standards | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||
Resistencia a la tracción | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | H19 | ||
185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | H19 | AA Standards |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H19 | ||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | H19 | ||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H19 | AA Standards | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H19 | AA Standards | |
Conductividad térmica | 230.0 W/(m·K) Show Material materials with Conductividad térmica of 230.0 W/(m·K) | H19 | ||
234 W/(m·K) Show Material materials with Conductividad térmica of 234 W/(m·K) | H19 | AA Standards | ||
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H19 | AA Standards | |
650.0 °C Show Material materials with Temperatura de fusión of 650.0 °C | H19 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 36000000.0 S/m Show Material materials with Conductividad eléctrica of 36000000.0 S/m | H19 | AA Standards |
Resistividad eléctrica | 2.78e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.78e-08 Ω·m | H19 | AA Standards |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 99.5 % Show Material materials with Aluminio of 99.5 % | H19 | AA Standards |
99.5 - 100.0 % Show Material materials with Aluminio of 99.5 - 100.0 % | H19 | ||
Boro | 0.05 % Show Material materials with Boro of 0.05 % | H19 | AA Standards |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H19 | AA Standards |
Cromo | 0.01 % Show Material materials with Cromo of 0.01 % | H19 | AA Standards |
Galio | 0.03 % Show Material materials with Galio of 0.03 % | H19 | AA Standards |
Hierro | 0.40 % Show Material materials with Hierro of 0.40 % | H19 | AA Standards |
0.4 % Show Material materials with Hierro of 0.4 % | H19 | ||
Manganeso | 0.01 % Show Material materials with Manganeso of 0.01 % | H19 | AA Standards |
Otro | 0.1 % Show Material materials with Otro of 0.1 % | H19 | |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % | H19 | AA Standards |
Titanio | 0.02 % Show Material materials with Titanio of 0.02 % | H19 | |
Vanadio | 0.02 % Show Material materials with Vanadio of 0.02 % | H19 | |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | H19 | AA Standards |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12, H111), poor (H14, H24, H16, H26, H18) | |
Workability | general (condition): good (O, H12, H111, H14, H24), acceptable (H16, H26, H18) |