General
Property | Value | Condition |
---|---|---|
Densidad | 3.1 g/cm³ Show Material materials with Densidad of 3.1 g/cm³ | T4 |
Mecánica
Property | Value | Condition | Comment |
---|---|---|---|
Charpy impact energy, V-notch | 21.7 J Show Material materials with Charpy impact energy, V-notch of 21.7 J | T4 | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | T4 | |
Dureza Brinell | 95 [-] Show Material materials with Dureza Brinell of 95 [-] | T4 | 500 kg load, 10 mm b |
Elongación | 20.0 % Show Material materials with Elongación of 20.0 % | T4 | |
20 % Show Material materials with Elongación of 20 % | T4 | Sand cast, elongation in 50 mm | |
Límite elástico | 215 MPa Show Material materials with Límite elástico of 215 MPa | T4 | Sand cast, RP02 |
220.0 MPa Show Material materials with Límite elástico of 220.0 MPa | T4 | ||
Módulo de cizallamiento | 23.0 GPa Show Material materials with Módulo de cizallamiento of 23.0 GPa | T4 | |
Módulo elástico | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | T4 | |
71 GPa Show Material materials with Módulo elástico of 71 GPa | T4 | ||
Resistencia a la tracción | 365 MPa Show Material materials with Resistencia a la tracción of 365 MPa | T4 | Sand cast |
370.0 MPa Show Material materials with Resistencia a la tracción of 370.0 MPa | T4 |
Aplicaciones térmicas
Property | Value | Condition |
---|---|---|
Calor específico | 920.0 J/(kg·K) Show Material materials with Calor específico of 920.0 J/(kg·K) | T4 |
Coeficiente de dilatación térmica | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T4 |
Conductividad térmica | 120.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 W/(m·K) | T4 |
Temperatura de fusión | 570.0 °C Show Material materials with Temperatura de fusión of 570.0 °C | T4 |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 16000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 23000000.0 S/m | Typical for Cast 2xx.x Series Aluminium |
Resistividad eléctrica | 4.347826086956522e-08 - 6.25e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.347826086956522e-08 - 6.25e-08 Ω·m | Typical for Cast 2xx.x Series Aluminium |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminio | 92.1 - 95.1 % Show Material materials with Aluminio of 92.1 - 95.1 % | T4 |
Cobre | 4.0 - 5.2 % Show Material materials with Cobre of 4.0 - 5.2 % | T4 |
Hierro | 0.15 % Show Material materials with Hierro of 0.15 % | T4 |
Magnesio | 0.15 - 0.55 % Show Material materials with Magnesio of 0.15 - 0.55 % | T4 |
Manganeso | 0.2 - 0.5 % Show Material materials with Manganeso of 0.2 - 0.5 % | T4 |
Otro | 0.1 % Show Material materials with Otro of 0.1 % | T4 |
Plata | 0.4 - 1.0 % Show Material materials with Plata of 0.4 - 1.0 % | T4 |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % | T4 |
Titanio | 0.15 - 0.35 % Show Material materials with Titanio of 0.15 - 0.35 % | T4 |