General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.79 g/cm³ Show Material materials with Densidad of 2.79 g/cm³ | O | AA Standards, ASTM B211, ASTM B316 |
2.79 g/cm³ Show Material materials with Densidad of 2.79 g/cm³ | O | ||
3.0 g/cm³ Show Material materials with Densidad of 3.0 g/cm³ | O |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 90.0 MPa Show Material materials with Bending Fatigue Strength of 90.0 MPa | O | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Dureza Brinell | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | O | AA Standards | |
45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | O | 500 kg load, 10 mm ball | ||
Elongación | 14.0 % Show Material materials with Elongación of 14.0 % | O | AA Standards, ASTM B211 | A100 |
16.0 % Show Material materials with Elongación of 16.0 % | O | AA Standards, ASTM B211 | A50 | |
19.0 % Show Material materials with Elongación of 19.0 % | O | |||
20.0 % Show Material materials with Elongación of 20.0 % | O | AA Standards | A100 | |
22 % Show Material materials with Elongación of 22 % | O | |||
Límite elástico | 70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | O | AA Standards | RP02 |
70 MPa Show Material materials with Límite elástico of 70 MPa | O | RP02 | ||
76.0 MPa Show Material materials with Límite elástico of 76.0 MPa | O | |||
Módulo de cizallamiento | 27.5 GPa Show Material materials with Módulo de cizallamiento of 27.5 GPa | O | ||
Módulo elástico | 72 GPa Show Material materials with Módulo elástico of 72 GPa | O | ||
73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | O | AA Standards, ASTM B211, ASTM B316 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Resistencia a la tracción | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | O | AA Standards | |
180 MPa Show Material materials with Resistencia a la tracción of 180 MPa | O | |||
190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | O | |||
240.0 MPa Show Material materials with Resistencia a la tracción of 240.0 MPa | O | AA Standards, ASTM B211, ASTM B316 | ||
Resistencia al cizallamiento | 125.0 MPa Show Material materials with Resistencia al cizallamiento of 125.0 MPa | O |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 870.0 J/(kg·K) Show Material materials with Calor específico of 870.0 J/(kg·K) | O | |||
Coeficiente de dilatación térmica | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | O | |||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | AA Standards, ASTM B211, ASTM B316 | ||
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | AA Standards, ASTM B211, ASTM B316 | ||
Conductividad térmica | 134.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 134.0 - 193.0 W/(m·K) | O | AA Standards, ASTM B211, ASTM B316 | ||
190.0 W/(m·K) Show Material materials with Conductividad térmica of 190.0 W/(m·K) | O | ||||
20 °C | 193 W/(m·K) Show Material materials with Conductividad térmica of 193 W/(m·K) | O | unstated value | ||
Temperatura de fusión | 510.0 - 640.0 °C Show Material materials with Temperatura de fusión of 510.0 - 640.0 °C | O | AA Standards, ASTM B211, ASTM B316 | ||
510.0 °C Show Material materials with Temperatura de fusión of 510.0 °C | O |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 20000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 29000000.0 S/m | O | AA Standards, ASTM B211, ASTM B316 | |
29000000 S/m Show Material materials with Conductividad eléctrica of 29000000 S/m | O | Typical/derived value | ||
Resistividad eléctrica | 3.45e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 5e-08 Ω·m | O | AA Standards, ASTM B211, ASTM B316 | |
3.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.5e-08 Ω·m | O | Typical value | ||
Specific Electrical conductivity | 50.0 % IACS Show Material materials with Specific Electrical conductivity of 50.0 % IACS | O | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 91.6 - 95.5 % Show Material materials with Aluminio of 91.6 - 95.5 % | O | |
Cobre | 3.5 - 4.5 % Show Material materials with Cobre of 3.5 - 4.5 % | O | AA Standards, ASTM B211, ASTM B316 |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | O | AA Standards, ASTM B211, ASTM B316 |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | O | AA Standards, ASTM B211, ASTM B316 |
0.7 % Show Material materials with Hierro of 0.7 % | O | ||
Magnesio | 0.4 - 0.8 % Show Material materials with Magnesio of 0.4 - 0.8 % | O | AA Standards, ASTM B211, ASTM B316 |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | O | AA Standards, ASTM B211, ASTM B316 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | O | |
Silicona | 0.2 - 0.8 % Show Material materials with Silicona of 0.2 - 0.8 % | O | AA Standards, ASTM B211, ASTM B316 |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | O | AA Standards, ASTM B211, ASTM B316 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | AA Standards, ASTM B211, ASTM B316 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: sufficient, in principle it should be protected | |
General machinability | General: good to acceptable | |
Workability | general (condition): poor(T4, T451) |