General
Property | Value |
---|---|
Densidad | 8.8 g/cm³ Show Supplier Material materials with Densidad of 8.8 g/cm³ |
Medidas
Property | Value |
---|---|
Dimensions | Strip thickness 0.08 - 3.0 mm, other gauges on request. Strip width from 8.5 mm. Hot-dip tinned and electroplated strip available. |
Mecánica
Property | Value | Testing Standard | Comment |
---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Supplier Material materials with Coeficiente de Poisson of 0.33 [-] | ||
Dureza Vickers | 110 - 140 [-] Show Supplier Material materials with Dureza Vickers of 110 - 140 [-] | R365(1/2H) | For reference only | |
125 - 145 [-] Show Supplier Material materials with Dureza Vickers of 125 - 145 [-] | R415(H) | For reference only | ||
130 - 150 [-] Show Supplier Material materials with Dureza Vickers of 130 - 150 [-] | R460(EH) | For reference only | ||
135 - 155 [-] Show Supplier Material materials with Dureza Vickers of 135 - 155 [-] | R480(SH) | For reference only | ||
150 [-] Show Supplier Material materials with Dureza Vickers of 150 [-] | min. | R530(XSH) | For reference only | ||
155 [-] Show Supplier Material materials with Dureza Vickers of 155 [-] | min. | R550(SSH) | For reference only | ||
Elongación | 1 % Show Supplier Material materials with Elongación of 1 % | min. | R530(XSH), A50 | |
1 % Show Supplier Material materials with Elongación of 1 % | min. | R550(SSH), A50 | ||
2 % Show Supplier Material materials with Elongación of 2 % | min. | R460(EH), A50 | ||
2 % Show Supplier Material materials with Elongación of 2 % | min. | R480(SH), A50 | ||
3 % Show Supplier Material materials with Elongación of 3 % | min. | R415(H), A50 | ||
6 % Show Supplier Material materials with Elongación of 6 % | min. | R365(1/2H), A50 | ||
Límite elástico | 250 MPa Show Supplier Material materials with Límite elástico of 250 MPa | min. | R365(1/2H) | |
365 MPa Show Supplier Material materials with Límite elástico of 365 MPa | min. | R415(H) | ||
440 MPa Show Supplier Material materials with Límite elástico of 440 MPa | min. | R460(EH) | ||
460 MPa Show Supplier Material materials with Límite elástico of 460 MPa | min. | R480(SH) | ||
500 MPa Show Supplier Material materials with Límite elástico of 500 MPa | min. | R530(XSH) | ||
520 MPa Show Supplier Material materials with Límite elástico of 520 MPa | min. | R550(SSH) | ||
Módulo elástico | 121 GPa Show Supplier Material materials with Módulo elástico of 121 GPa | ||
Plegabilidad 180 ° bidireccional | 1 [-] Show Supplier Material materials with Plegabilidad 180 ° bidireccional of 1 [-] | ASTM B820 | R365(1/2H) | bending thickness: <0.5 mm & bending width: 10 mm |
1.5 [-] Show Supplier Material materials with Plegabilidad 180 ° bidireccional of 1.5 [-] | ASTM B820 | R415(H) | bending thickness: <0.5 mm & bending width: 10 mm | |
1.5 [-] Show Supplier Material materials with Plegabilidad 180 ° bidireccional of 1.5 [-] | ASTM B820 | R460(EH) | bending thickness: <0.5 mm & bending width: 10 mm | |
2 [-] Show Supplier Material materials with Plegabilidad 180 ° bidireccional of 2 [-] | ASTM B820 | R480(SH) | bending thickness: <0.5 mm & bending width: 10 mm | |
Plegabilidad 180 ° en peso bruto | 1 [-] Show Supplier Material materials with Plegabilidad 180 ° en peso bruto of 1 [-] | ASTM B820 | R365(1/2H) | bending thickness: <0.5 mm & bending width: 10 mm |
1.5 [-] Show Supplier Material materials with Plegabilidad 180 ° en peso bruto of 1.5 [-] | ASTM B820 | R415(H) | bending thickness: <0.5 mm & bending width: 10 mm | |
1.5 [-] Show Supplier Material materials with Plegabilidad 180 ° en peso bruto of 1.5 [-] | ASTM B820 | R460(EH) | bending thickness: <0.5 mm & bending width: 10 mm | |
2 [-] Show Supplier Material materials with Plegabilidad 180 ° en peso bruto of 2 [-] | ASTM B820 | R480(SH) | bending thickness: <0.5 mm & bending width: 10 mm | |
Plegabilidad 90 ° bidireccional | 0 [-] Show Supplier Material materials with Plegabilidad 90 ° bidireccional of 0 [-] | EN ISO 7438 | R365(1/2H) | bending thickness: <0.5 mm & bending width: 10 mm |
0.5 [-] Show Supplier Material materials with Plegabilidad 90 ° bidireccional of 0.5 [-] | EN ISO 7438 | R415(H) | bending thickness: <0.5 mm & bending width: 10 mm | |
1 [-] Show Supplier Material materials with Plegabilidad 90 ° bidireccional of 1 [-] | EN ISO 7438 | R460(EH) | bending thickness: <0.5 mm & bending width: 10 mm | |
1.2 [-] Show Supplier Material materials with Plegabilidad 90 ° bidireccional of 1.2 [-] | EN ISO 7438 | R480(SH) | bending thickness: <0.5 mm & bending width: 10 mm | |
2 [-] Show Supplier Material materials with Plegabilidad 90 ° bidireccional of 2 [-] | EN ISO 7438 | R530(XSH) | bending thickness: <0.5 mm & bending width: 10 mm | |
Plegabilidad 90 ° en peso bruto | 0 [-] Show Supplier Material materials with Plegabilidad 90 ° en peso bruto of 0 [-] | EN ISO 7438 | R365(1/2H) | bending thickness: <0.5 mm & bending width: 10 mm |
0.5 [-] Show Supplier Material materials with Plegabilidad 90 ° en peso bruto of 0.5 [-] | EN ISO 7438 | R415(H) | bending thickness: <0.5 mm & bending width: 10 mm | |
0.5 [-] Show Supplier Material materials with Plegabilidad 90 ° en peso bruto of 0.5 [-] | EN ISO 7438 | R460(EH) | bending thickness: <0.5 mm & bending width: 10 mm | |
0.8 [-] Show Supplier Material materials with Plegabilidad 90 ° en peso bruto of 0.8 [-] | EN ISO 7438 | R480(SH) | bending thickness: <0.5 mm & bending width: 10 mm | |
1.5 [-] Show Supplier Material materials with Plegabilidad 90 ° en peso bruto of 1.5 [-] | EN ISO 7438 | R530(XSH) | bending thickness: <0.5 mm & bending width: 10 mm | |
Resistencia a la tracción | 365 - 435 MPa Show Supplier Material materials with Resistencia a la tracción of 365 - 435 MPa | R365(1/2H) | |
415 - 485 MPa Show Supplier Material materials with Resistencia a la tracción of 415 - 485 MPa | R415(H) | ||
460 - 505 MPa Show Supplier Material materials with Resistencia a la tracción of 460 - 505 MPa | R460(EH) | ||
485 - 525 MPa Show Supplier Material materials with Resistencia a la tracción of 485 - 525 MPa | R480(SH) |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 385 J/(kg·K) Show Supplier Material materials with Calor específico of 385 J/(kg·K) | ||
Coeficiente de dilatación térmica | 1.76e-05 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.76e-05 1/K | average value between 20-300°C | |
Conductividad térmica | 20 °C | 280 W/(m·K) Show Supplier Material materials with Conductividad térmica of 280 W/(m·K) |
Eléctrico
Chemical properties
Technological properties
Property | ||
---|---|---|
Application areas | Application target: Ideal for semiconductor. | |
Chemical composition | The chemical composition is the nominal composition of the alloy | |
Coating | Electroplating: Good Hot dip tinning: Very good | |
Cold Forming | Good | |
Machining | Not suitable | |
Packaging size | Standard coils with outside diameters up to 1300 mm. Traverse-wound coils with drum weights up to 500 kg. Multiple-coil up to 3 tons. | |
Testings | Fatigue strength: The fatigue strength is defined as the maximum bending stress amplitude which a material withstands for 10.000.000 load cycles under symmetrical alternate load without breaking. It depends on the temper selected and can be estimated typically by 1/3 of tensile strength. For solid solution fine grain materials fatigue strength might increase up to 0,5 * of tensile strength. Bending test: 90° bend test According to EN ISO 7438, 180° bend test acc. to ASTM B820, shown values might show orange- peel, however no crack. | |
Welding | Laser welding: Good Resistance welding: Good |