General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 10.2 g/cm³ Show Supplier Material materials with Densidad of 10.2 g/cm³ |
Medidas
Property | Value |
---|---|
Diámetro | 0.5 - 0.8 mm Show Supplier Material materials with Diámetro of 0.5 - 0.8 mm |
Dimensions | Available diameters (mm): 0.5; 0.4; 0.6; 0.7; 0.8 |
Mecánica
Property | Temperature | Value |
---|---|---|
Elongación | 23.0 °C | 10 % Show Supplier Material materials with Elongación of 10 % |
Resistencia a la tracción | 23.0 °C | 970 - 1150 MPa Show Supplier Material materials with Resistencia a la tracción of 970 - 1150 MPa |
Aplicaciones térmicas
Property | Value |
---|---|
Temperatura de cristalización | 1700 °C Show Supplier Material materials with Temperatura de cristalización of 1700 °C |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminio | 1E-4 % Show Supplier Material materials with Aluminio of 1E-4 % | ||
Cadmio | 1E-4 % Show Supplier Material materials with Cadmio of 1E-4 % | ||
Carbono | 1.3E-3 % Show Supplier Material materials with Carbono of 1.3E-3 % | ||
Cobre | 2E-4 % Show Supplier Material materials with Cobre of 2E-4 % | ||
Cromo | 3E-4 % Show Supplier Material materials with Cromo of 3E-4 % | ||
Hierro | 5E-4 % Show Supplier Material materials with Hierro of 5E-4 % | ||
Lantano | 0.19 - 0.31 % Show Supplier Material materials with Lantano of 0.19 - 0.31 % | as La | |
Molibdeno | balance | ||
Nitrógeno | 5E-4 % Show Supplier Material materials with Nitrógeno of 5E-4 % | ||
Níquel | 1E-4 % Show Supplier Material materials with Níquel of 1E-4 % | ||
Otro | 0.22 - 0.36 % Show Supplier Material materials with Otro of 0.22 - 0.36 % | as La₂O₃ | |
Potasio | 6E-4 % Show Supplier Material materials with Potasio of 6E-4 % | ||
Silicona | 2E-4 % Show Supplier Material materials with Silicona of 2E-4 % | ||
Wolframio | 0.02 % Show Supplier Material materials with Wolframio of 0.02 % |
Technological properties
Property | ||
---|---|---|
Application areas | This alloy is mostly machined to produce furnace components such as stranded and other wires, sintering and annealing boats or evaporator coils. In the lighting industry, molybdenum-lanthanum oxide is used, for example, for retaining and feed wires. |