Property | Temperature | Value | Thickness | Testing Standard | Condition | Comment |
---|---|---|---|---|---|---|
Absorción de agua | 6 % Show Supplier Material materials with Absorción de agua of 6 % | 2 mm | ISO 62 | immersion at 23°C | ||
Densidad | 1.22 g/cm³ Show Supplier Material materials with Densidad of 1.22 g/cm³ | ISO 1183 | dry | |||
Moisture absorption | 23 °C | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | 2 mm | ISO 62 | 50%RH |
Mecánica
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elongación | 2.3 % Show Supplier Material materials with Elongación of 2.3 % | dry | ISO 527-2/1A | 5mm/min | |
3.5 % Show Supplier Material materials with Elongación of 3.5 % | 50%RH | ISO 527-2/1A | 5mm/min | ||
Módulo de flexión | 13.5 GPa Show Supplier Material materials with Módulo de flexión of 13.5 GPa | dry | ISO 178 | 2mm/min | |
Módulo elástico | 10.2 GPa Show Supplier Material materials with Módulo elástico of 10.2 GPa | 50%RH | ISO 527-2/1A | 1mm/min | |
16.5 GPa Show Supplier Material materials with Módulo elástico of 16.5 GPa | dry | ISO 527-2/1A | 1mm/min | ||
Resistencia a la flexión | 310 MPa Show Supplier Material materials with Resistencia a la flexión of 310 MPa | dry | ISO 178 | 2mm/min | |
Resistencia a la tracción | 150 MPa Show Supplier Material materials with Resistencia a la tracción of 150 MPa | 50%RH | ISO 527-2/1A | 5mm/min | |
215 MPa Show Supplier Material materials with Resistencia a la tracción of 215 MPa | dry | ISO 527-2/1A | 5mm/min | ||
Resistencia al choque, ensayo Charpy no entallado | 23 °C | 50 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 50 kJ/m² | dry | ISO 179/1eU | |
23 °C | 75 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 75 kJ/m² | 50%RH | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Thickness | Testing Standard | Comment | |||
---|---|---|---|---|---|---|---|
Temperatura de fusión | 260 °C Show Supplier Material materials with Temperatura de fusión of 260 °C | 1000 mm | ISO 11357-1/-3 | 10°C/min | |||
Inflamabilidad | Class: HB, Standard: UL 94 | Automotive Interior Flammability(mm/min): <10 ,method: ISO 3795 and thickness tested (mm): 3 |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Volume resistivity | 100 Ω·cm Show Supplier Material materials with Volume resistivity of 100 Ω·cm | dry, 50%RH | IEC 60093 | 500V |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Features | Increased Electrical Conductivity | |
Fillers | 20% Carbon Fiber | |