General
Property | Temperature | Value | Thickness | Testing Standard | Condition | Comment |
---|---|---|---|---|---|---|
Absorción de agua | 3.2 % Show Supplier Material materials with Absorción de agua of 3.2 % | 2 mm | ISO 62 | immersion at 23°C | ||
Densidad | 1.08 g/cm³ Show Supplier Material materials with Densidad of 1.08 g/cm³ | ISO 1183 | dry | |||
Moisture absorption | 23 °C | 1.4 % Show Supplier Material materials with Moisture absorption of 1.4 % | 2 mm | ISO 62 | 50%RH |
Mecánica
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elongación | 40 % Show Supplier Material materials with Elongación of 40 % | dry | ISO 527-2/1A | 50mm/min | nominal | |
100 % Show Supplier Material materials with Elongación of 100 % | 50%RH | ISO 527-2/1A | min. | 50mm/min | nominal | ||
Elongation at yield | 4.6 % Show Supplier Material materials with Elongation at yield of 4.6 % | dry | ISO 527-2/1A | 50mm/min | |
15 % Show Supplier Material materials with Elongation at yield of 15 % | 50%RH | ISO 527-2/1A | 50mm/min | ||
Límite elástico | 45 MPa Show Supplier Material materials with Límite elástico of 45 MPa | 50%RH | ISO 527-2/1A | 50mm/min | |
65 MPa Show Supplier Material materials with Límite elástico of 65 MPa | dry | ISO 527-2/1A | 50mm/min | ||
Módulo de flexión | 2.2 GPa Show Supplier Material materials with Módulo de flexión of 2.2 GPa | dry | ISO 178 | 2mm/min | |
Módulo elástico | 1.3 GPa Show Supplier Material materials with Módulo elástico of 1.3 GPa | 50%RH | ISO 527-2/1A | 1mm/min | |
2.4 GPa Show Supplier Material materials with Módulo elástico of 2.4 GPa | dry | ISO 527-2/1A | 1mm/min | ||
Resistencia a la flexión | 85 MPa Show Supplier Material materials with Resistencia a la flexión of 85 MPa | dry | ISO 178 | 2mm/min | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 4.5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 4.5 kJ/m² | dry | ISO 179/1eA | |
-30 °C | 7.5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 7.5 kJ/m² | 50%RH | ISO 179/1eA | ||
23 °C | 5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 5 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | 50%RH | ISO 179/1eA | ||
Resistencia al choque, ensayo Charpy no entallado | No Break at 23°C | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Testing Standard | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 0.00011 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.00011 1/K | ISO 11359-1/-2 | 23°C-55°C | ||
0.00011 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.00011 1/K | ISO 11359-1/-2 | 23°C-55°C, Transverse | |||
Temperatura de flexión bajo carga | 65 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 65 °C | ISO 75/2Af | 1.80 MPa | ||
160 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 160 °C | ISO 75/2Bf | 0.45 MPa | |||
Temperatura de fusión | 220 °C Show Supplier Material materials with Temperatura de fusión of 220 °C | ISO 11357-1/-3 | 10°C/min | ||
Temperatura de reblandecimiento Vicat | 185 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 185 °C | ISO 306 | 50°C/h 50N | ||
Inflamabilidad | Thickness tested (mm): 0.8, Class: HB, Standard: UL 94 |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Surface resistivity | 1e+10 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+10 Ω/sq | 50%RH | IEC 60093 | 500V |
1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | dry | IEC 60093 | 500V | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | 50%RH | IEC 60093 | 500V |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 1 % Show Supplier Material materials with Contracción of 1 % | 270/60/60* | ISO 294-4 | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa] |
1.2 % Show Supplier Material materials with Contracción of 1.2 % | 270/60/60* | ISO 294-4 | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa], Transverse |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Deep black | |
Features | Heat Stabilized | |
Processing methods | Injection Molding |