General
Property | Value | Thickness | Testing Standard | Condition | Comment |
---|---|---|---|---|---|
Absorción de agua | 0.7 % Show Supplier Material materials with Absorción de agua of 0.7 % | 2 mm | ISO 62 | 24h immersion at 23°C | |
1.9 % Show Supplier Material materials with Absorción de agua of 1.9 % | 2 mm | ISO 62 | immersion at 23°C | ||
Densidad | 1.27 g/cm³ Show Supplier Material materials with Densidad of 1.27 g/cm³ | ISO 1183 | dry |
Mecánica
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elongación | 20 % Show Supplier Material materials with Elongación of 20 % | dry | ISO 527-2/1A | 50mm/min | nominal | |
Elongation at yield | 11 % Show Supplier Material materials with Elongation at yield of 11 % | dry | ISO 527-2/1A | 50mm/min | |
Límite elástico | 61 MPa Show Supplier Material materials with Límite elástico of 61 MPa | dry | ISO 527-2/1A | 50mm/min | |
Módulo de flexión | 3.1 GPa Show Supplier Material materials with Módulo de flexión of 3.1 GPa | dry | ISO 178 | 2mm/min | |
Módulo elástico | 3.2 GPa Show Supplier Material materials with Módulo elástico of 3.2 GPa | dry | ISO 527-2/1A | 1mm/min | |
Resistencia a la flexión | 95 MPa Show Supplier Material materials with Resistencia a la flexión of 95 MPa | dry | ISO 178 | 2mm/min | |
Resistencia al choque, ensayo Charpy entallado | 23 °C | 4.2 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 4.2 kJ/m² | dry | ISO 179/1eA |
Aplicaciones térmicas
Property | Value | Testing Standard | Comment |
---|---|---|---|
Temperatura de fusión | 213 °C Show Supplier Material materials with Temperatura de fusión of 213 °C | ISO 11357-1/-3 | 10°C/min |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 1.1 % Show Supplier Material materials with Contracción of 1.1 % | 280/60/60* | ISO 294-4 | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa], Transverse |
1.2 % Show Supplier Material materials with Contracción of 1.2 % | 280/60/60* | ISO 294-4 | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa] |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | Food Contact, Drinking Water, RoHS 2011/65/UE | |
Color | Black | |
Features | Hydrolysis Resistance | |
Fillers | 30% Glass Bead | |
Processing methods | Injection Molding |