General
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Alargamiento A2 | 23.0 °C | 35 % Show Supplier Material materials with Alargamiento A2 of 35 % | min. |
Creep strength 10^4 cycles | 525.0 °C | 155 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 155 MPa | at 10000h, average values |
550.0 °C | 133 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 133 MPa | at 10000h, average values | |
575.0 °C | 113 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 113 MPa | at 10000h, average values | |
600.0 °C | 96 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 96 MPa | at 10000h, average values | |
625.0 °C | 81 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 81 MPa | at 10000h, average values | |
650.0 °C | 68 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 68 MPa | at 10000h, average values | |
675.0 °C | 55 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 55 MPa | at 10000h, average values | |
700.0 °C | 44 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 44 MPa | at 10000h, average values | |
725.0 °C | 36 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 36 MPa | at 10000h, average values | |
750.0 °C | 30 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 30 MPa | at 10000h, average values | |
775.0 °C | 25 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 25 MPa | at 10000h, average values | |
800.0 °C | 21 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 21 MPa | at 10000h, average values | |
825.0 °C | 18 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 18 MPa | at 10000h, average values | |
850.0 °C | 15 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 15 MPa | at 10000h, average values | |
875.0 °C | 12 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 12 MPa | at 10000h, average values | |
900.0 °C | 10 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 10 MPa | at 10000h, average values | |
925.0 °C | 8 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 8 MPa | at 10000h, average values | |
950.0 °C | 6 MPa Show Supplier Material materials with Creep strength 10^4 cycles of 6 MPa | at 10000h, average values | |
Creep strength 10^5 cycles | 525.0 °C | 105 - 155 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 105 - 155 MPa | at 100000h, average values |
550.0 °C | 85 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 85 MPa | at 100000h, average values | |
575.0 °C | 68 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 68 MPa | at 100000h, average values | |
600.0 °C | 56 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 56 MPa | at 100000h, average values | |
625.0 °C | 45 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 45 MPa | at 100000h, average values | |
650.0 °C | 36 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 36 MPa | at 100000h, average values | |
675.0 °C | 29 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 29 MPa | at 100000h, average values | |
700.0 °C | 24 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 24 MPa | at 100000h, average values | |
725.0 °C | 20 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 20 MPa | at 100000h, average values | |
750.0 °C | 17 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 17 MPa | at 100000h, average values | |
775.0 °C | 14 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 14 MPa | at 100000h, average values | |
800.0 °C | 11 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 11 MPa | at 100000h, average values | |
825.0 °C | 9 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 9 MPa | at 100000h, average values | |
850.0 °C | 7 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 7 MPa | at 100000h, average values | |
875.0 °C | 5 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 5 MPa | at 100000h, average values | |
900.0 °C | 4 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 4 MPa | at 100000h, average values | |
925.0 °C | 4 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 4 MPa | at 100000h, average values | |
950.0 °C | 3 MPa Show Supplier Material materials with Creep strength 10^5 cycles of 3 MPa | at 100000h, average values | |
Dureza Rockwell B | 23.0 °C | 90 [-] Show Supplier Material materials with Dureza Rockwell B of 90 [-] | max. |
Elongación | 23.0 °C | 35 % Show Supplier Material materials with Elongación of 35 % | min. |
Límite elástico Rp 0,2 | 20.0 °C | 220 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 220 MPa | min. |
50.0 °C | 213 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 213 MPa | min. | |
100.0 °C | 192 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 192 MPa | min. | |
150.0 °C | 176 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 176 MPa | min. | |
200.0 °C | 161 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 161 MPa | min. | |
250.0 °C | 150 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 150 MPa | min. | |
300.0 °C | 141 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 141 MPa | min. | |
350.0 °C | 134 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 134 MPa | min. | |
400.0 °C | 129 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 129 MPa | min. | |
450.0 °C | 125 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 125 MPa | min. | |
500.0 °C | 123 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 123 MPa | min. | |
550.0 °C | 121 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 121 MPa | min. | |
Límite elástico Rp0.1 | 20.0 °C | 250 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 250 MPa | min. |
50.0 °C | 238 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 238 MPa | min. | |
100.0 °C | 217 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 217 MPa | min. | |
150.0 °C | 201 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 201 MPa | min. | |
200.0 °C | 186 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 186 MPa | min. | |
250.0 °C | 175 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 175 MPa | min. | |
300.0 °C | 166 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 166 MPa | min. | |
350.0 °C | 159 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 159 MPa | min. | |
400.0 °C | 154 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 154 MPa | min. | |
450.0 °C | 150 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 150 MPa | min. | |
500.0 °C | 148 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 148 MPa | min. | |
550.0 °C | 146 MPa Show Supplier Material materials with Límite elástico Rp0.1 of 146 MPa | min. | |
Módulo elástico | 20.0 °C | 195 GPa Show Supplier Material materials with Módulo elástico of 195 GPa | |
100.0 °C | 190 GPa Show Supplier Material materials with Módulo elástico of 190 GPa | ||
200.0 °C | 182 GPa Show Supplier Material materials with Módulo elástico of 182 GPa | ||
300.0 °C | 174 GPa Show Supplier Material materials with Módulo elástico of 174 GPa | ||
400.0 °C | 166 GPa Show Supplier Material materials with Módulo elástico of 166 GPa | ||
500.0 °C | 158 GPa Show Supplier Material materials with Módulo elástico of 158 GPa | ||
Resistencia a la tracción | 23.0 °C | 530 - 750 MPa Show Supplier Material materials with Resistencia a la tracción of 530 - 750 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 470 J/(kg·K) Show Supplier Material materials with Calor específico of 470 J/(kg·K) | |
100.0 °C | 495 J/(kg·K) Show Supplier Material materials with Calor específico of 495 J/(kg·K) | ||
200.0 °C | 530 J/(kg·K) Show Supplier Material materials with Calor específico of 530 J/(kg·K) | ||
300.0 °C | 555 J/(kg·K) Show Supplier Material materials with Calor específico of 555 J/(kg·K) | ||
400.0 °C | 580 J/(kg·K) Show Supplier Material materials with Calor específico of 580 J/(kg·K) | ||
500.0 °C | 600 J/(kg·K) Show Supplier Material materials with Calor específico of 600 J/(kg·K) | ||
600.0 °C | 615 J/(kg·K) Show Supplier Material materials with Calor específico of 615 J/(kg·K) | ||
700.0 °C | 630 J/(kg·K) Show Supplier Material materials with Calor específico of 630 J/(kg·K) | ||
Coeficiente de dilatación térmica | 100.0 °C | 1.55E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.55E-5 1/K | for 20°C to the mentioned temperature |
200.0 °C | 1.5E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.5E-5 1/K | for 20°C to the mentioned temperature | |
300.0 °C | 1.55E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.55E-5 1/K | for 20°C to the mentioned temperature | |
400.0 °C | 1.6E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.6E-5 1/K | for 20°C to the mentioned temperature | |
500.0 °C | 1.65E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.65E-5 1/K | for 20°C to the mentioned temperature | |
600.0 °C | 1.7E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K | for 20°C to the mentioned temperature | |
700.0 °C | 1.75E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.75E-5 1/K | for 20°C to the mentioned temperature | |
800.0 °C | 1.85E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.85E-5 1/K | for 20°C to the mentioned temperature | |
900.0 °C | 1.9E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.9E-5 1/K | for 20°C to the mentioned temperature | |
1000.0 °C | 1.9E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.9E-5 1/K | for 20°C to the mentioned temperature | |
Conductividad térmica | 20.0 °C | 13 W/(m·K) Show Supplier Material materials with Conductividad térmica of 13 W/(m·K) | |
100.0 °C | 15 W/(m·K) Show Supplier Material materials with Conductividad térmica of 15 W/(m·K) | ||
200.0 °C | 17 W/(m·K) Show Supplier Material materials with Conductividad térmica of 17 W/(m·K) | ||
300.0 °C | 19 W/(m·K) Show Supplier Material materials with Conductividad térmica of 19 W/(m·K) | ||
400.0 °C | 21 W/(m·K) Show Supplier Material materials with Conductividad térmica of 21 W/(m·K) | ||
500.0 °C | 23 W/(m·K) Show Supplier Material materials with Conductividad térmica of 23 W/(m·K) | ||
600.0 °C | 25 W/(m·K) Show Supplier Material materials with Conductividad térmica of 25 W/(m·K) | ||
700.0 °C | 26 W/(m·K) Show Supplier Material materials with Conductividad térmica of 26 W/(m·K) | ||
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Azufre | 0.015 % Show Supplier Material materials with Azufre of 0.015 % | max. | |
Carbono | 0.06 % Show Supplier Material materials with Carbono of 0.06 % | max. | |
Cromo | 24.5 % Show Supplier Material materials with Cromo of 24.5 % | ||
Fósforo | 0.03 % Show Supplier Material materials with Fósforo of 0.03 % | max. | |
Hierro | Balance | ||
Manganeso | 1.5 % Show Supplier Material materials with Manganeso of 1.5 % | max. | |
Níquel | 21 % Show Supplier Material materials with Níquel of 21 % | ||
Silicona | 0.75 % Show Supplier Material materials with Silicona of 0.75 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | The good, general high temperature corrosion resistance of Sandvik 7RE10 makes it suitable for a wide range of applications: | |
Cold Forming | Annealing after cold bending is not normally necessary, but this should be reviewed depending on the degree of bending and the operating conditions. Heat treatment, if any, should take the form of stress relieving or solution annealing. See under "Heat treatment". Solution annealing is recommended for tubes used at temperatures above 750°C (1380°F), and when the highest possible creep strength is required in the bent tube. | |
Corrosion properties | Sandvik 7RE10 has very good resistance to oxidation and sulphidation. It can be used in: The high chromium content of Sandvik 7RE10 makes the material resistant to oxidizing aqueous solutions. Sandvik 7RE10 also has better resistance to chloride induced stress corrosion cracking than lower alloyed steels of type ASTM 304 and 316. Sandvik 7RE10 has good resistance in cyanide melts and neutral salts melts at high temperature. The material is insensitive to "green rot" attack. | |
Heat Treatment | Tubes are generally delivered in the solution annealed condition. If another heat treatment is needed after further processing the following is recommended: Stress relieving: 850-950°C (1560-1740°F), 10-15 minutes, cooling in air. The temperature should not be allowed to fall below 850°C (1560°F), because of the risk of sensitization. Solution annealing: 1000-1150°C (1830-2100°F), 5-20 minutes, rapid cooling in air or water. | |
Hot forming | Hot bending is carried out at 1100-850°C (2010-1560°F) and should be followed by solution annealing. | |
Other | Forms of supply: Seamless tube and pipe in Sandvik 7RE10 is supplied in dimensions up to 260 mm outside diameter, in the solution annealed and white-pickled condition or in the bright annealed condition. Stock sizes: Sandvik 7RE10 is stocked in sizes ranging from 13.5 mm to 168.28 mm (6") outside diameter. Additional data concerning sizes and finishes is available on request from your nearest Sandvik office. | |
Structural Stability | Like other austenitic stainless steels, Sandvik 7RE10 has better structural stability than high alloyed ferritic steels. At temperatures between 800 and 900°C (1470-1650°F), however, the structural stability will be slightly impaired. For service in this temperature range, we recommend the use of Sanicro 31HT, which has better structural stability. | |
Welding | The weldability of Sandvik 7RE10 is good. Suitable methods of fusion welding are manual metal-arc welding (MMA/SMAW) and gas-shielded arc welding, with the TIG/GTAW method as first choice. In common with all fully austenitic stainless steels, Sandvik 7RE10 has low thermal conductivity and high thermal expansion. Welding plans should therefore be carefully selected in advance, so that distortions of the welded joint are minimized. If residual stresses are a concern, solution annealing can be performed after welding. Welding of fully austenitic stainless steel can entail the risk of hot cracking in the welded joints, particularly under high constraint. For Sandvik 7RE10, heat-input of <1.0 kJ/mm and interpass temperature of <100°C (210°F) are recommended. A string bead welding technique should be used. Recommended filler metals:
|