DIN 1712-3 Grade 3.0205 F

Want to keep this datasheet? Save it now in your required format

Description

Pure aluminium This material is well anodically oxidizable and has a good electrical and thermal conductivity. The splinter-giving workability is bad because of danger of smearing. Its mechanical strength is low, the plasticity high. The forming capacity and the chemical as well as weather proofness are excellent. The materialist it for welding and braze welding well suitably. Application: Apparatus engineering, roll bond, z-bond, household devices, camp and tansport tanks for the chemical, pharmaceutical and food industry, roofings, linings, arts and crafts, packing, flow pressed parts (tubes, tube, doses, bottles), metal goods, motor vehicle characteristics.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM,AluKey.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

2.71 g/cm³

Show Material materials with Densidad of 2.71 g/cm³

F

EN 573-3, EN 485, EN 570, EN 755

20.0 °C

2.71 g/cm³

Show Material materials with Densidad of 2.71 g/cm³

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Dureza Brinell

25.0 [-]

Show Material materials with Dureza Brinell of 25.0 [-]

F

EN 573-3, EN 570

20.0 °C

22.0 [-]

Show Material materials with Dureza Brinell of 22.0 [-]

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Elongación

18.0 %

Show Material materials with Elongación of 18.0 %

F

EN 573-3, EN 755

A50

20.0 %

Show Material materials with Elongación of 20.0 %

F

EN 573-3, EN 755

A100

20.0 °C

16.0 %

Show Material materials with Elongación of 16.0 %

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

A10

20.0 °C

18.0 %

Show Material materials with Elongación of 18.0 %

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Módulo de cizallamiento

25.9 GPa

Show Material materials with Módulo de cizallamiento of 25.9 GPa

F

EN 573-3, EN 485, EN 570, EN 755

20.0 °C

24.0 - 26.0 GPa

Show Material materials with Módulo de cizallamiento of 24.0 - 26.0 GPa

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Módulo elástico

69.0 GPa

Show Material materials with Módulo elástico of 69.0 GPa

F

EN 573-3, EN 485, EN 570, EN 755

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Módulo elástico of 60.0 - 65.0 GPa

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Resistencia a la tracción

75.0 MPa

Show Material materials with Resistencia a la tracción of 75.0 MPa

F

EN 573-3, EN 485, EN 755

20.0 °C

75.0 MPa

Show Material materials with Resistencia a la tracción of 75.0 MPa

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShapeComment

Calor específico

900.0 - 963.0 J/(kg·K)

Show Material materials with Calor específico of 900.0 - 963.0 J/(kg·K)

Typical for Wrought 1000 Series Aluminium

Coeficiente de dilatación térmica

-50 °C

2.17e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755, DIN 1712-3, EN 573-4

Profile, Rod, Tube

-50.0 °C

2.17e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755, DIN 1712-3, EN 573-4

Profile, Rod, Tube

20 °C

2.17e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755, DIN 1712-3, EN 573-4

Profile, Rod, Tube

20 °C

2.35e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755, DIN 1712-3, EN 573-4

Profile, Rod, Tube

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755

100 °C

2.35e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755, DIN 1712-3, EN 573-4

Profile, Rod, Tube

100.0 °C

2.35e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755, DIN 1712-3, EN 573-4

Profile, Rod, Tube

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755

200.0 °C

2.44e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.44e-05 1/K

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K

F

EN 573-3, EN 485, EN 570, EN 755

300.0 °C

2.54e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.54e-05 1/K

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Conductividad térmica

20.0 °C

205.0 - 210.0 W/(m·K)

Show Material materials with Conductividad térmica of 205.0 - 210.0 W/(m·K)

F

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 570, EN 755

Profile, Rod, Tube

Temperatura de fusión

644.0 - 657.0 °C

Show Material materials with Temperatura de fusión of 644.0 - 657.0 °C

F

EN 573-3, EN 485, EN 570, EN 755

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShape

Conductividad eléctrica

33000000.0 - 34000000.0 S/m

Show Material materials with Conductividad eléctrica of 33000000.0 - 34000000.0 S/m

F

EN 573-3, EN 485, EN 570, EN 755

20.0 °C

34400000.0 - 35500000.0 S/m

Show Material materials with Conductividad eléctrica of 34400000.0 - 35500000.0 S/m

F

DIN 1712-3, EN 573-3, EN 573-4

Profile, Rod, Tube

Resistividad eléctrica

2.94e-08 - 3.03e-08 Ω·m

Show Material materials with Resistividad eléctrica of 2.94e-08 - 3.03e-08 Ω·m

F

EN 573-3, EN 485, EN 570, EN 755

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminio

99.0 %

Show Material materials with Aluminio of 99.0 %

F

EN 573-3, EN 485, EN 570, EN 755

Cobre

0.05 %

Show Material materials with Cobre of 0.05 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 570, EN 755

Profile, Rod, Tube

Magnesio

0.05 %

Show Material materials with Magnesio of 0.05 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 570, EN 755

Profile, Rod, Tube

Manganeso

0.05 %

Show Material materials with Manganeso of 0.05 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 570, EN 755

Profile, Rod, Tube

Titanio

0.05 %

Show Material materials with Titanio of 0.05 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 570, EN 755

Profile, Rod, Tube

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

F

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 570, EN 755

Profile, Rod, Tube

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: sufficient, weathering: acceptable

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12)