General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | |
Elongación | 20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | A10 | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Módulo de cizallamiento | 20.0 °C | 25.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 26.5 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
Módulo elástico | -195.0 °C | 78.4 GPa Show Material materials with Módulo elástico of 78.4 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
-85.0 °C | 73.5 GPa Show Material materials with Módulo elástico of 73.5 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
-30.0 °C | 71.4 GPa Show Material materials with Módulo elástico of 71.4 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Módulo elástico of 60.0 - 70.0 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
100.0 °C | 68.6 GPa Show Material materials with Módulo elástico of 68.6 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
150.0 °C | 66.5 GPa Show Material materials with Módulo elástico of 66.5 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
250.0 °C | 56.0 GPa Show Material materials with Módulo elástico of 56.0 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | |
20.0 °C | 150.0 - 190.0 MPa Show Material materials with Resistencia a la tracción of 150.0 - 190.0 MPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Flat |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
Coeficiente de dilatación térmica | -50.0 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
100.0 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.44e-05 1/K | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.54e-05 1/K | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
Conductividad térmica | 20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 210.0 - 220.0 W/(m·K) | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
Temperatura de fusión | 645.0 - 660.0 °C Show Material materials with Temperatura de fusión of 645.0 - 660.0 °C | Typical for Wrought 1000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 34800000.0 - 36000000.0 S/m Show Material materials with Conductividad eléctrica of 34800000.0 - 36000000.0 S/m | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
Resistividad eléctrica | 2.7e-08 - 3e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.7e-08 - 3e-08 Ω·m | Typical for Wrought 1000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 Show Material materials with Cobre of 0.05 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Hierro | 0.4 Show Material materials with Hierro of 0.4 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Magnesio | 0.05 Show Material materials with Magnesio of 0.05 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Manganeso | 0.05 Show Material materials with Manganeso of 0.05 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Silicona | 0.25 Show Material materials with Silicona of 0.25 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Titanio | 0.05 Show Material materials with Titanio of 0.05 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Zinc | 0.07 Show Material materials with Zinc of 0.07 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |