General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 65.0 MPa Show Material materials with Bending Fatigue Strength of 65.0 MPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Dureza Brinell | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | H14 | EN 573-3, EN 485 | |||
20.0 °C | 35.0 [-] Show Material materials with Dureza Brinell of 35.0 [-] | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Tube, Wire | ||
20.0 °C | 40.0 [-] Show Material materials with Dureza Brinell of 40.0 [-] | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod | ||
20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | ||
Elongación | -196.0 °C | 27.0 % Show Material materials with Elongación of 27.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | ||
-80.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
-20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3, EN 683 | A50 | |||
2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3, EN 485 | A50 | |||
3.0 % Show Material materials with Elongación of 3.0 % | H14 | EN 573-3, EN 485 | A50 | |||
4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3, EN 485, EN 754 | A50 | |||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 1301 | ||||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 485 | A100 | |||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 485 | A50 | |||
6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3, EN 754 | A100 | |||
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Wire | A100 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | A10 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Tube, Wire | A10 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Tube | ||
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | H14 | DIN 1725-1 | Strip | A50 Transverse | |
100.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
150.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
200.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
260.0 °C | 60.0 % Show Material materials with Elongación of 60.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
320.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
370.0 °C | 70.0 % Show Material materials with Elongación of 70.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | |||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire | ||
Módulo elástico | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | -196.0 °C | 253.0 MPa Show Material materials with Resistencia a la tracción of 253.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | ||
-80.0 °C | 172.0 MPa Show Material materials with Resistencia a la tracción of 172.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
-20.0 °C | 158.0 MPa Show Material materials with Resistencia a la tracción of 158.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
130.0 - 165.0 MPa Show Material materials with Resistencia a la tracción of 130.0 - 165.0 MPa | H14 | EN 573-3, EN 754 | ||||
135.0 - 180.0 MPa Show Material materials with Resistencia a la tracción of 135.0 - 180.0 MPa | H14 | EN 573-3, EN 1301 | ||||
20.0 °C | 90.0 - 140.0 MPa Show Material materials with Resistencia a la tracción of 90.0 - 140.0 MPa | H14 | DIN 1725-1 | Strip | Transverse | |
20.0 °C | 130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Tube, Wire | ||
20.0 °C | 140.0 - 180.0 MPa Show Material materials with Resistencia a la tracción of 140.0 - 180.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 485, EN 683 | Sheet, Strip | ||
20.0 °C | 155.0 MPa Show Material materials with Resistencia a la tracción of 155.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
100.0 °C | 148.0 MPa Show Material materials with Resistencia a la tracción of 148.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
150.0 °C | 127.0 MPa Show Material materials with Resistencia a la tracción of 127.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
200.0 °C | 98.0 MPa Show Material materials with Resistencia a la tracción of 98.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
260.0 °C | 53.0 MPa Show Material materials with Resistencia a la tracción of 53.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
320.0 °C | 28.0 MPa Show Material materials with Resistencia a la tracción of 28.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
370.0 °C | 19.0 MPa Show Material materials with Resistencia a la tracción of 19.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
Resistencia al cizallamiento | 20.0 °C | 75.0 MPa Show Material materials with Resistencia al cizallamiento of 75.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Wire | |
Ángulo de flexión a 180° | 2.0 °/t Show Material materials with Ángulo de flexión a 180° of 2.0 °/t | H14 | EN 573-3, EN 485 | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H14 | EN 573-3, EN 485 | ||||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H14 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire | |
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
Conductividad térmica | 20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 28000000.0 S/m | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Resistividad eléctrica | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.57e-08 - 4.55e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 683, EN 754 | Strip, Rod, Sheet, Tube, Wire |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 683, EN 754 | Strip, Rod, Sheet, Tube, Wire |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Strip, Rod, Sheet, Tube, Wire |
0.70 % Show Material materials with Hierro of 0.70 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 683, EN 754 | Strip, Rod, Sheet, Tube, Wire |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 683, EN 754 | Strip, Rod, Sheet, Tube, Wire |
Titanio | 0.1 Show Material materials with Titanio of 0.1 | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 683, EN 754 | Strip, Rod, Sheet, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |