DIN 1725-1 Grade 3.0525 H12

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMn1Mg0,5 is similarly to AlMn1 in its properties. It reaches strength up to F 25. The alloy belongs to the nature-hard aluminum materials. A strength increase can only occure by cold forming. It is very well hot and cold formable and is suitable to the deep-drawing (no lappet formation). The alloy AlMn1Mg0,5 is very well corrosion resistant and is sea water steady. As semi-finished material it is present in accordance with DIN 1788 and DIN 1745 only as sheet metal or strip. Application: Mainly in the packing for cans (lower parts), for menu bowls, for covers. In the building industry for claddings, roofings, for sun protection facilities (roller schutter, lamella net curtain) and for roll gates as well as for flexible pipes and in the construction of vehicles.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM,AluKey.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

2.72 g/cm³

Show Material materials with Densidad of 2.72 g/cm³

H12

EN 573-3, EN 485

20.0 °C

2.72 g/cm³

Show Material materials with Densidad of 2.72 g/cm³

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Dureza Brinell

46.0 [-]

Show Material materials with Dureza Brinell of 46.0 [-]

H12

EN 573-3, EN 485

20.0 °C

50.0 [-]

Show Material materials with Dureza Brinell of 50.0 [-]

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Elongación

3.0 %

Show Material materials with Elongación of 3.0 %

H12

EN 573-3, EN 485

A50

4.0 %

Show Material materials with Elongación of 4.0 %

H12

EN 573-3, EN 485

A50

5.0 %

Show Material materials with Elongación of 5.0 %

H12

EN 573-3, EN 485

A50

20.0 °C

5.0 %

Show Material materials with Elongación of 5.0 %

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

A10

20.0 °C

6.0 %

Show Material materials with Elongación of 6.0 %

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Módulo de cizallamiento

20.0 °C

26.5

Show Material materials with Módulo de cizallamiento of 26.5

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Módulo elástico

70.0 GPa

Show Material materials with Módulo elástico of 70.0 GPa

H12

EN 573-3, EN 485

20.0 °C

65.0 GPa

Show Material materials with Módulo elástico of 65.0 GPa

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Resistencia a la tracción

145.0 - 195.0 MPa

Show Material materials with Resistencia a la tracción of 145.0 - 195.0 MPa

H12

EN 573-3, EN 485

20.0 °C

155.0 - 195.0 MPa

Show Material materials with Resistencia a la tracción of 155.0 - 195.0 MPa

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Ángulo de flexión a 180°

1.5 °/t

Show Material materials with Ángulo de flexión a 180° of 1.5 °/t

H12

EN 573-3, EN 485

2.0 °/t

Show Material materials with Ángulo de flexión a 180° of 2.0 °/t

H12

EN 573-3, EN 485

Ángulo de flexión a 90°

0.5 °/t

Show Material materials with Ángulo de flexión a 90° of 0.5 °/t

H12

EN 573-3, EN 485

1.0 °/t

Show Material materials with Ángulo de flexión a 90° of 1.0 °/t

H12

EN 573-3, EN 485

1.5 °/t

Show Material materials with Ángulo de flexión a 90° of 1.5 °/t

H12

EN 573-3, EN 485

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShape

Calor específico

20.0 °C

893.0 J/(kg·K)

Show Material materials with Calor específico of 893.0 J/(kg·K)

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Coeficiente de dilatación térmica

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K

H12

EN 573-3, EN 485

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K

H12

EN 573-3, EN 485

Conductividad térmica

160.0 - 190.0 W/(m·K)

Show Material materials with Conductividad térmica of 160.0 - 190.0 W/(m·K)

H12

EN 573-3, EN 485

20.0 °C

200.0 W/(m·K)

Show Material materials with Conductividad térmica of 200.0 W/(m·K)

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Temperatura de fusión

630.0 - 654.0 °C

Show Material materials with Temperatura de fusión of 630.0 - 654.0 °C

H12

EN 573-3, EN 485

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShape

Conductividad eléctrica

23000000.0 - 25000000.0 S/m

Show Material materials with Conductividad eléctrica of 23000000.0 - 25000000.0 S/m

H12

EN 573-3, EN 485

20.0 °C

28000000.0 S/m

Show Material materials with Conductividad eléctrica of 28000000.0 S/m

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

Resistividad eléctrica

4e-08 - 4.35e-08 Ω·m

Show Material materials with Resistividad eléctrica of 4e-08 - 4.35e-08 Ω·m

H12

EN 573-3, EN 485

Chemical properties

PropertyValueConditionRelated StandardsShape

Cobre

0.3 %

Show Material materials with Cobre of 0.3 %

H12

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet, Strip

Cromo

0.1 %

Show Material materials with Cromo of 0.1 %

H12

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet, Strip

Hierro

0.7 %

Show Material materials with Hierro of 0.7 %

H12

DIN 1725-1, EN 573-3, EN 573-4

Sheet, Strip

0.70 %

Show Material materials with Hierro of 0.70 %

H12

EN 573-3, EN 485

Magnesio

0.2 - 0.6 %

Show Material materials with Magnesio of 0.2 - 0.6 %

H12

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet, Strip

Manganeso

1.0 - 1.5 %

Show Material materials with Manganeso of 1.0 - 1.5 %

H12

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet, Strip

Silicona

0.6 %

Show Material materials with Silicona of 0.6 %

H12

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet, Strip

Titanio

0.1 %

Show Material materials with Titanio of 0.1 %

H12

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet, Strip

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H12

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet, Strip

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / acceptable (H12)