General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | O | EN 573-3, EN 485, EN 754, EN 755 | ||
20.0 °C | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 29.0 [-] Show Material materials with Dureza Brinell of 29.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 30.0 [-] Show Material materials with Dureza Brinell of 30.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube, Wire | ||
20.0 °C | 32.0 [-] Show Material materials with Dureza Brinell of 32.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elongación | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 485 | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 754 | A50 | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 754 | A100 | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 755 | A50 | |||
19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 485, EN 755 | A100 | |||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 485 | A50 | |||
22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3, EN 485 | A50 | |||
24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Wire | A10 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Tube | A10 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 21.0 % Show Material materials with Elongación of 21.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 24.0 % Show Material materials with Elongación of 24.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | O | EN 573-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 25.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Módulo elástico | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | O | EN 573-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 100.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 145.0 MPa | O | EN 573-3, EN 485, EN 754 | |||
100.0 - 150.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 150.0 MPa | O | EN 573-3, EN 755 | ||||
20.0 °C | 100.0 MPa Show Material materials with Resistencia a la tracción of 100.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube, Wire | ||
20.0 °C | 105.0 - 140.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 140.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 105.0 - 135.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 135.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Ángulo de flexión a 180° | 0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
Ángulo de flexión a 90° | 1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | |||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | O | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 879.0 J/(kg·K) Show Material materials with Calor específico of 879.0 J/(kg·K) | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Coeficiente de dilatación térmica | -50 °C | 2.18e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.18e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
-50.0 °C | 2.18e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.18e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20 °C | 2.18e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.18e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20 °C | 2.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.45e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20 °C | 2.55e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.55e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
100.0 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
200 °C | 2.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.45e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
200.0 °C | 2.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.45e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
300 °C | 2.55e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.55e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
300.0 °C | 2.55e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.55e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Conductividad térmica | 20.0 °C | 160.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 220.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Temperatura de fusión | 630.0 - 650.0 °C Show Material materials with Temperatura de fusión of 630.0 - 650.0 °C | O | EN 573-3, EN 485, EN 754, EN 755 | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 23000000.0 - 31000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 31000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Resistividad eléctrica | 3.23e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.23e-08 - 4.35e-08 Ω·m | O | EN 573-3, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
0.2 % Show Material materials with Cobre of 0.2 % | O | EN 573-3, EN 485, EN 754, EN 755 | ||
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Hierro | 0.45 % Show Material materials with Hierro of 0.45 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
0.70 % Show Material materials with Hierro of 0.70 % | O | EN 573-3, EN 485, EN 754, EN 755 | ||
Magnesio | 0.7 - 1.1 % Show Material materials with Magnesio of 0.7 - 1.1 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
1.1 - 1.8 % Show Material materials with Magnesio of 1.1 - 1.8 % | O | EN 573-3, EN 485, EN 754, EN 755 | ||
Manganeso | 0.15 % Show Material materials with Manganeso of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
0.3 % Show Material materials with Manganeso of 0.3 % | O | EN 573-3, EN 485, EN 754, EN 755 | ||
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
0.4 % Show Material materials with Silicona of 0.4 % | O | EN 573-3, EN 485, EN 754, EN 755 | ||
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
0.25 % Show Material materials with Zinc of 0.25 % | O | EN 573-3, EN 485, EN 754, EN 755 |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |