The AlMg alloy is characterised all by a good corrosion resistance. It is sea water steady and resistant to saline atmosphere. The Mg content increase the strength, the cold forming capacity decreases with it. The alloys of this type are nature hard, i.e. only by a cold forming and not by a purposeful heat treatment a strength increase can be attained. The material is well polishabel and anodisable. The splinter-giving machinability becomes better with increasing Mg content just like the weldability. The alloy AlMg1 reaches strength grades to F 22. Application: Their main field of application is the building industry. In the building industry for claddings, roofing and trim, for transport containers. For metal goods, like building fittings, table-ware, flow pressed parts, reflectors. In food industry, for furniture (incl. camping furniture) as well as for describe and for covers with composite slabs (intermediate layer: Polyethylene).

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM,AluKey.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

2.69 g/cm³

Show Material materials with Densidad of 2.69 g/cm³

H28

EN 573-3, EN 485

20.0 °C

2.69 g/cm³

Show Material materials with Densidad of 2.69 g/cm³

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Dureza Brinell

58.0 [-]

Show Material materials with Dureza Brinell of 58.0 [-]

H28

EN 573-3, EN 485

20.0 °C

57.0 [-]

Show Material materials with Dureza Brinell of 57.0 [-]

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Elongación

1.0 %

Show Material materials with Elongación of 1.0 %

H28

EN 573-3, EN 485

A50

2.0 %

Show Material materials with Elongación of 2.0 %

H28

EN 573-3, EN 485

A50

3.0 %

Show Material materials with Elongación of 3.0 %

H28

EN 573-3, EN 485

A50

20.0 °C

4.0 %

Show Material materials with Elongación of 4.0 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

A10

20.0 °C

5.0 %

Show Material materials with Elongación of 5.0 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Módulo de cizallamiento

26.1 GPa

Show Material materials with Módulo de cizallamiento of 26.1 GPa

H28

EN 573-3, EN 485

20.0 °C

25.0 GPa

Show Material materials with Módulo de cizallamiento of 25.0 GPa

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Módulo elástico

69.5 GPa

Show Material materials with Módulo elástico of 69.5 GPa

H28

EN 573-3, EN 485

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Módulo elástico of 60.0 - 65.0 GPa

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Resistencia a la tracción

185.0 MPa

Show Material materials with Resistencia a la tracción of 185.0 MPa

H28

EN 573-3, EN 485

20.0 °C

190.0 MPa

Show Material materials with Resistencia a la tracción of 190.0 MPa

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Ángulo de flexión a 90°

1.5 °/t

Show Material materials with Ángulo de flexión a 90° of 1.5 °/t

H28

EN 573-3, EN 485

2.5 °/t

Show Material materials with Ángulo de flexión a 90° of 2.5 °/t

H28

EN 573-3, EN 485

3.0 °/t

Show Material materials with Ángulo de flexión a 90° of 3.0 °/t

H28

EN 573-3, EN 485

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShapeComment

Calor específico

20.0 °C

879.0 J/(kg·K)

Show Material materials with Calor específico of 879.0 J/(kg·K)

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Coeficiente de dilatación térmica

-50 °C

2.18e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.18e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

-50.0 °C

2.18e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.18e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

20 °C

2.18e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.18e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

20 °C

2.36e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

20 °C

2.45e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.45e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

20 °C

2.55e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.55e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

100 °C

2.36e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

100.0 °C

2.36e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

200 °C

2.45e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.45e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

200.0 °C

2.45e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.45e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

300 °C

2.55e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.55e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

300.0 °C

2.55e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.55e-05 1/K

H28

EN 573-3, EN 485, DIN 1725-1, EN 573-4

Sheet

Conductividad térmica

20.0 °C

160.0 - 220.0 W/(m·K)

Show Material materials with Conductividad térmica of 160.0 - 220.0 W/(m·K)

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet

Temperatura de fusión

630.0 - 650.0 °C

Show Material materials with Temperatura de fusión of 630.0 - 650.0 °C

H28

EN 573-3, EN 485

Temperatura máx. de funcionamiento

150.0 °C

Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShape

Conductividad eléctrica

20.0 °C

23000000.0 - 31000000.0 S/m

Show Material materials with Conductividad eléctrica of 23000000.0 - 31000000.0 S/m

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet

Resistividad eléctrica

3.23e-08 - 4.35e-08 Ω·m

Show Material materials with Resistividad eléctrica of 3.23e-08 - 4.35e-08 Ω·m

H28

EN 573-3, EN 485

Chemical properties

PropertyValueConditionRelated StandardsShape

Cobre

0.05 %

Show Material materials with Cobre of 0.05 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

0.2 %

Show Material materials with Cobre of 0.2 %

H28

EN 573-3, EN 485

Cromo

0.1 %

Show Material materials with Cromo of 0.1 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485

Sheet

Hierro

0.45 %

Show Material materials with Hierro of 0.45 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

0.70 %

Show Material materials with Hierro of 0.70 %

H28

EN 573-3, EN 485

Magnesio

0.7 - 1.1 %

Show Material materials with Magnesio of 0.7 - 1.1 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

1.1 - 1.8 %

Show Material materials with Magnesio of 1.1 - 1.8 %

H28

EN 573-3, EN 485

Manganeso

0.15 %

Show Material materials with Manganeso of 0.15 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

0.3 %

Show Material materials with Manganeso of 0.3 %

H28

EN 573-3, EN 485

Silicona

0.3 %

Show Material materials with Silicona of 0.3 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

0.4 %

Show Material materials with Silicona of 0.4 %

H28

EN 573-3, EN 485

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Sheet

0.25 %

Show Material materials with Zinc of 0.25 %

H28

EN 573-3, EN 485

Technological properties

Property
Workability

Good workability.