General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H28 | EN 573-3, EN 485 | ||
2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H28 | EN 573-3, EN 485 | |||
20.0 °C | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 67.0 [-] Show Material materials with Dureza Brinell of 67.0 [-] | H28 | EN 573-3, EN 485 | |||
20.0 °C | 65.0 [-] Show Material materials with Dureza Brinell of 65.0 [-] | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | H28 | EN 573-3, EN 485 | A50 | ||
2.0 % Show Material materials with Elongación of 2.0 % | H28 | EN 573-3, EN 485 | A50 | |||
3.0 % Show Material materials with Elongación of 3.0 % | H28 | EN 573-3, EN 485 | A50 | |||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Módulo de cizallamiento | 20.0 °C | 26.5 Show Material materials with Módulo de cizallamiento of 26.5 | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H28 | EN 573-3, EN 485 | |||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H28 | EN 573-3, EN 485 | ||||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | H28 | EN 573-3, EN 485 | |||
20.0 °C | 225.0 MPa Show Material materials with Resistencia a la tracción of 225.0 MPa | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Ángulo de flexión a 90° | 1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H28 | EN 573-3, EN 485 | |||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H28 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 879.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H28 | EN 573-3, EN 485 | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H28 | EN 573-3, EN 485 | |||
Conductividad térmica | 170.0 - 190.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 190.0 W/(m·K) | H28 | EN 573-3, EN 485 | |||
193 W/(m·K) Show Material materials with Conductividad térmica of 193 W/(m·K) | H28 | EN 573-3, EN 485 | ||||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Temperatura de fusión | 620.0 - 650.0 °C Show Material materials with Temperatura de fusión of 620.0 - 650.0 °C | H28 | EN 573-3, EN 485 | |||
625.0 - 650.0 °C Show Material materials with Temperatura de fusión of 625.0 - 650.0 °C | H28 | EN 573-3, EN 485 | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 23000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 26000000.0 S/m | H28 | EN 573-3, EN 485 | ||
29000000.0 S/m Show Material materials with Conductividad eléctrica of 29000000.0 S/m | H28 | EN 573-3, EN 485 | |||
20.0 °C | 28000000.0 - 30000000.0 S/m Show Material materials with Conductividad eléctrica of 28000000.0 - 30000000.0 S/m | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Resistividad eléctrica | 3.45e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 Ω·m | H28 | EN 573-3, EN 485 | ||
3.85e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 - 4.35e-08 Ω·m | H28 | EN 573-3, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H28 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Flat |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H28 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Flat |
Hierro | 0.45 % Show Material materials with Hierro of 0.45 % | H28 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
0.45 % Show Material materials with Hierro of 0.45 % | H28 | EN 573-3, EN 485 | ||
Magnesio | 1.1 - 1.7 % Show Material materials with Magnesio of 1.1 - 1.7 % | H28 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Flat |
Manganeso | 0.15 % Show Material materials with Manganeso of 0.15 % | H28 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Flat |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H28 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Flat |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H28 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Flat |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |