General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20.0 °C | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 30.0 [-] Show Material materials with Dureza Brinell of 30.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | |
Elongación | 20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | A10 | |
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Módulo de cizallamiento | 20.0 °C | 26.0 Show Material materials with Módulo de cizallamiento of 26.0 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | |
Módulo elástico | 20.0 °C | 70.0 Show Material materials with Módulo elástico of 70.0 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 100.0 - 140.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 140.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | |
20.0 °C | 100.0 MPa Show Material materials with Resistencia a la tracción of 100.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 879.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium |
Coeficiente de dilatación térmica | 2.2e-05 - 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium |
Conductividad térmica | 112.0 - 205.0 W/(m·K) Show Material materials with Conductividad térmica of 112.0 - 205.0 W/(m·K) | Typical for Wrought 5000 Series Aluminium |
Temperatura de fusión | 560.0 - 655.0 °C Show Material materials with Temperatura de fusión of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium |
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 33000000.0 Show Material materials with Conductividad eléctrica of 33000000.0 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | |
Resistividad eléctrica | 3.3e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Hierro | 0.08 Show Material materials with Hierro of 0.08 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Magnesio | 0.7 - 1.1 % Show Material materials with Magnesio of 0.7 - 1.1 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Manganeso | 0.03 Show Material materials with Manganeso of 0.03 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Silicona | 0.08 Show Material materials with Silicona of 0.08 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Titanio | 0.02 Show Material materials with Titanio of 0.02 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Zinc | 0.05 Show Material materials with Zinc of 0.05 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |