WL 3.3354 Grade 3.3354 F

Want to keep this datasheet? Save it now in your required format

Description

The alloy is characterised by a good corrosion resistance. It is sea water steady and resistant to saline atmosphere. The Mg content increases the strength, but the cold forming capacity decreases. The material is nature hard, i.e. only by a cold forming and not by a purposeful heat treatment a strength increase can be attained. It is well polishable and anodisable. The splinter-giving machinability becomes better with increasing Mg content, just as the weldability. AlMg5 has the highest Mg content of the standardized AlMg alloys, so it is badly cold formable, but the strength is the highest, so that the employment is possible for statically more highly loaded constructions. The alloy is suitable for a splinter-giving machinig on automats. It possesses sensitivity to intergranular corrosion. By a purposeful heat treatment and/or by additive of Mn or Cr the inclination to the intergranular corrosion can be reduced. Application: In the optics, in the automobile engineering for body parts, in mechanical engineering (turned parts). For joining elements (solid rivets, blind rivets, riveting nuts and screws). In the building industry for carrying constructions as well as in shipbuilding considering the sensitivity to corrosion.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

20.0 °C

2.64 g/cm³

Show Material materials with Densidad of 2.64 g/cm³

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Dureza Brinell

20.0 °C

55.0 [-]

Show Material materials with Dureza Brinell of 55.0 [-]

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile

20.0 °C

60.0 [-]

Show Material materials with Dureza Brinell of 60.0 [-]

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Rod

20.0 °C

65.0 [-]

Show Material materials with Dureza Brinell of 65.0 [-]

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Tube

Elongación

20.0 °C

10.0 %

Show Material materials with Elongación of 10.0 %

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging

20.0 °C

11.0 %

Show Material materials with Elongación of 11.0 %

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Profile, Rod, Tube

A10

20.0 °C

12.0 %

Show Material materials with Elongación of 12.0 %

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging

20.0 °C

13.0 %

Show Material materials with Elongación of 13.0 %

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Profile, Rod, Tube

Módulo de cizallamiento

20.0 °C

27.0 GPa

Show Material materials with Módulo de cizallamiento of 27.0 GPa

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Módulo elástico

20.0 °C

67.0 - 72.0 GPa

Show Material materials with Módulo elástico of 67.0 - 72.0 GPa

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Resistencia a la tracción

20.0 °C

240.0 MPa

Show Material materials with Resistencia a la tracción of 240.0 MPa

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging

20.0 °C

250.0 MPa

Show Material materials with Resistencia a la tracción of 250.0 MPa

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Profile, Rod, Tube

20.0 °C

260.0 MPa

Show Material materials with Resistencia a la tracción of 260.0 MPa

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShapeComment

Calor específico

20.0 °C

904.0 J/(kg·K)

Show Material materials with Calor específico of 904.0 J/(kg·K)

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Coeficiente de dilatación térmica

-50.0 °C

2.25e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.25e-05 1/K

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

100.0 °C

2.41e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

200.0 °C

2.51e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.51e-05 1/K

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

300.0 °C

2.61e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.61e-05 1/K

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Conductividad térmica

20.0 °C

110.0 - 140.0 W/(m·K)

Show Material materials with Conductividad térmica of 110.0 - 140.0 W/(m·K)

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Temperatura de fusión

560.0 - 655.0 °C

Show Material materials with Temperatura de fusión of 560.0 - 655.0 °C

Typical for Wrought 5000 Series Aluminium

Temperatura máx. de funcionamiento

150.0 °C

Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShapeComment

Conductividad eléctrica

20.0 °C

15000000.0 - 19000000.0 S/m

Show Material materials with Conductividad eléctrica of 15000000.0 - 19000000.0 S/m

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Resistividad eléctrica

3.3e-08 - 5e-08 Ω·m

Show Material materials with Resistividad eléctrica of 3.3e-08 - 5e-08 Ω·m

Typical for Wrought 5000 Series Aluminium

Chemical properties

PropertyValueConditionRelated StandardsShape

Cobre

0.1

Show Material materials with Cobre of 0.1

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Cromo

0.2

Show Material materials with Cromo of 0.2

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Hierro

0.5

Show Material materials with Hierro of 0.5

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Magnesio

4.5 - 5.6 %

Show Material materials with Magnesio of 4.5 - 5.6 %

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Manganeso

0.1 - 0.6 %

Show Material materials with Manganeso of 0.1 - 0.6 %

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Silicona

0.4

Show Material materials with Silicona of 0.4

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Titanio

0.2

Show Material materials with Titanio of 0.2

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Zinc

0.2

Show Material materials with Zinc of 0.2

F

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Forging, Profile, Rod, Tube

Technological properties

Property
Workability

Good workability.