General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | O | EN 573-3, EN 485, EN 754 | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | O | EN 573-3, EN 754 | |||
52.0 [-] Show Material materials with Dureza Brinell of 52.0 [-] | O | EN 573-3, EN 485 | ||||
20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Strip, Sheet | ||
Elongación | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 485 | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 485 | A50 | |||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 754 | A50 | |||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 485 | A50 | |||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 485, EN 754 | A100 | |||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod | A10 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Tube | A10 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Strip, Sheet | ||
Módulo de cizallamiento | 20.0 °C | 26.5 Show Material materials with Módulo de cizallamiento of 26.5 | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube | |
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 485, EN 754 | |||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 180.0 - 250.0 MPa Show Material materials with Resistencia a la tracción of 180.0 - 250.0 MPa | O | EN 573-3, EN 754 | |||
190.0 - 240.0 MPa Show Material materials with Resistencia a la tracción of 190.0 - 240.0 MPa | O | EN 573-3, EN 485 | ||||
20.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 190.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 190.0 - 230.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Strip, Sheet | ||
Ángulo de flexión a 180° | 0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | O | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 879.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3699999999999997e-05 1/K | O | EN 573-3, EN 485, EN 754 | ||
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3699999999999997e-05 1/K | O | EN 573-3, EN 485, EN 754 | |||
Conductividad térmica | 20.0 °C | 140.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 - 180.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube | |
Temperatura de fusión | 620.0 - 650.0 °C Show Material materials with Temperatura de fusión of 620.0 - 650.0 °C | O | EN 573-3, EN 485, EN 754 | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube | Long | |
150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 20000000.0 - 25000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 25000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Resistividad eléctrica | 4e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4e-08 - 5e-08 Ω·m | O | EN 573-3, EN 485, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube |
0.50 % Show Material materials with Hierro of 0.50 % | O | EN 573-3, EN 485, EN 754 | ||
Magnesio | 1.6 - 2.5 % Show Material materials with Magnesio of 1.6 - 2.5 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Manganeso | 0.5 - 1.1 % Show Material materials with Manganeso of 0.5 - 1.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754 | Rod, Sheet, Strip, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |