DIN 1725-1 Grade 3.3527 H18

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMg2Mn0,8 has similar characteristics as the alloy AlMg1,8. The additive of Mn (>0,6%) causes an increase of the heat resistance (up to 150°C) of the material and the recrystallisation limit. The result of the last is, that in case of extruded profiles the strength in longitudinal direction increases. The material is characterised by a good corrosion resistance. It is sea water steady and steady against saline atmosphere. With the Mg content the strength increases, the cold forming capacity decreases. The alloy is nature hard, i.e. that only by a cold forming shaping however by a purposeful heat treatment a strength increase cannot be attained. The splinter-giving workability and the weldability are improved with increasing Mg content. Application: In the apparatus engineering for receivers accordint to AD-W6/1 and according to VdTUEV-Werkstoffblaetter, for compressed gas tanks (pipings), for very low-temperature tanks and for temperatures to 250 °C. In the automobile engineering for utilizable superstructures, silo trucks, in shipbuilding for trunk and superstructures. In the building industry for roofings, claddings, for carrying constructions according to DIN 4173 and sun protection facilities as well as for furniture (including camping furniture).

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM,AluKey.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

2.71 g/cm³

Show Material materials with Densidad of 2.71 g/cm³

H18

EN 573-3, EN 1592, EN 485, EN 754

20.0 °C

2.71 g/cm³

Show Material materials with Densidad of 2.71 g/cm³

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.33 [-]

Show Material materials with Coeficiente de Poisson of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Dureza Brinell

88.0 [-]

Show Material materials with Dureza Brinell of 88.0 [-]

H18

EN 573-3, EN 485

20.0 °C

85.0 [-]

Show Material materials with Dureza Brinell of 85.0 [-]

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

Elongación

1.0 %

Show Material materials with Elongación of 1.0 %

H18

EN 573-3, EN 485, EN 754

A50

2.0 %

Show Material materials with Elongación of 2.0 %

H18

EN 573-3, EN 754

A100

2.0 %

Show Material materials with Elongación of 2.0 %

H18

EN 573-3, EN 485

A50

3.0 %

Show Material materials with Elongación of 3.0 %

H18

EN 573-3, EN 1592

A100

20.0 °C

2.0 %

Show Material materials with Elongación of 2.0 %

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

A10

20.0 °C

3.0 %

Show Material materials with Elongación of 3.0 %

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

Módulo de cizallamiento

20.0 °C

26.5

Show Material materials with Módulo de cizallamiento of 26.5

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

Módulo elástico

70.0 GPa

Show Material materials with Módulo elástico of 70.0 GPa

H18

EN 573-3, EN 1592, EN 485, EN 754

20.0 °C

70.0 GPa

Show Material materials with Módulo elástico of 70.0 GPa

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Resistencia a la tracción

220.0 MPa

Show Material materials with Resistencia a la tracción of 220.0 MPa

H18

EN 573-3, EN 1592

280.0 MPa

Show Material materials with Resistencia a la tracción of 280.0 MPa

H18

EN 573-3, EN 754

290.0 MPa

Show Material materials with Resistencia a la tracción of 290.0 MPa

H18

EN 573-3, EN 485

20.0 °C

290.0 MPa

Show Material materials with Resistencia a la tracción of 290.0 MPa

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShapeComment

Calor específico

879.0 - 963.0 J/(kg·K)

Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K)

Typical for Wrought 5000 Series Aluminium

Coeficiente de dilatación térmica

20 °C

2.3699999999999997e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.3699999999999997e-05 1/K

H18

EN 573-3, EN 1592, EN 485, EN 754

100 °C

2.3699999999999997e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 2.3699999999999997e-05 1/K

H18

EN 573-3, EN 1592, EN 485, EN 754

Conductividad térmica

20.0 °C

140.0 - 180.0 W/(m·K)

Show Material materials with Conductividad térmica of 140.0 - 180.0 W/(m·K)

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Temperatura de fusión

620.0 - 650.0 °C

Show Material materials with Temperatura de fusión of 620.0 - 650.0 °C

H18

EN 573-3, EN 1592, EN 485, EN 754

Temperatura máx. de funcionamiento

150.0 °C

Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

Long

150.0 °C

Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShape

Conductividad eléctrica

20.0 °C

20000000.0 - 25000000.0 S/m

Show Material materials with Conductividad eléctrica of 20000000.0 - 25000000.0 S/m

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Resistividad eléctrica

4e-08 - 5e-08 Ω·m

Show Material materials with Resistividad eléctrica of 4e-08 - 5e-08 Ω·m

H18

EN 573-3, EN 1592, EN 485, EN 754

Chemical properties

PropertyValueConditionRelated StandardsShape

Cobre

0.1 %

Show Material materials with Cobre of 0.1 %

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Cromo

0.3 %

Show Material materials with Cromo of 0.3 %

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Hierro

0.5 %

Show Material materials with Hierro of 0.5 %

H18

DIN 1725-1, EN 573-3, EN 573-4

Flat

0.50 %

Show Material materials with Hierro of 0.50 %

H18

EN 573-3, EN 1592, EN 485, EN 754

Magnesio

1.6 - 2.5 %

Show Material materials with Magnesio of 1.6 - 2.5 %

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Manganeso

0.5 - 1.1 %

Show Material materials with Manganeso of 0.5 - 1.1 %

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Silicona

0.4 %

Show Material materials with Silicona of 0.4 %

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Titanio

0.1 %

Show Material materials with Titanio of 0.1 %

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H18

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754

Flat

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)