General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20.0 °C | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
20.0 °C | 80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elongación | 20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | A10 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A10 | |
Módulo de cizallamiento | 20.0 °C | 27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Módulo elástico | 20.0 °C | 68.0 - 72.0 GPa Show Material materials with Módulo elástico of 68.0 - 72.0 GPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
20.0 °C | 265.0 - 305.0 MPa Show Material materials with Resistencia a la tracción of 265.0 - 305.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
Resistencia al cizallamiento | 20.0 °C | 135.0 MPa Show Material materials with Resistencia al cizallamiento of 135.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 963.0 J/(kg·K) Show Material materials with Calor específico of 963.0 J/(kg·K) | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Coeficiente de dilatación térmica | 100.0 °C | 2.39e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.39e-05 1/K | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Conductividad térmica | 20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 - 160.0 W/(m·K) | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Temperatura de fusión | 560.0 - 655.0 °C Show Material materials with Temperatura de fusión of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 20000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 23000000.0 S/m | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Resistividad eléctrica | 3.3e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 Show Material materials with Cobre of 0.1 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Cromo | 0.3 Show Material materials with Cromo of 0.3 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Hierro | 0.4 Show Material materials with Hierro of 0.4 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Magnesio | 2.6 - 3.6 % Show Material materials with Magnesio of 2.6 - 3.6 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Manganeso | 0.5 Show Material materials with Manganeso of 0.5 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Silicona | 0.4 Show Material materials with Silicona of 0.4 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Titanio | 0.15 Show Material materials with Titanio of 0.15 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Zinc | 0.2 Show Material materials with Zinc of 0.2 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |