General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
2.78 g/cm³ Show Material materials with Densidad of 2.78 g/cm³ | T3 | EN 573-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Sheet, Strip, Tube, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 140.0 MPa Show Material materials with Bending Fatigue Strength of 140.0 MPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | |||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 123.0 [-] Show Material materials with Dureza Brinell of 123.0 [-] | T3 | EN 573-3, EN 485 | |||
124.0 [-] Show Material materials with Dureza Brinell of 124.0 [-] | T3 | EN 573-3, EN 485 | ||||
20.0 °C | 105.0 [-] Show Material materials with Dureza Brinell of 105.0 [-] | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 110.0 [-] Show Material materials with Dureza Brinell of 110.0 [-] | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 115.0 [-] Show Material materials with Dureza Brinell of 115.0 [-] | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 120.0 [-] Show Material materials with Dureza Brinell of 120.0 [-] | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Tube | ||
20.0 °C | 125.0 [-] Show Material materials with Dureza Brinell of 125.0 [-] | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | ||
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T3 | EN 573-3, EN 755 | A50 | ||
7.0 % Show Material materials with Elongación of 7.0 % | T3 | EN 573-3, EN 754 | A50 | |||
8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3, EN 755 | A100 | |||
8.0 % Show Material materials with Elongación of 8.0 % | T3 | EN 573-3, EN 754 | A50 | |||
9.0 % Show Material materials with Elongación of 9.0 % | T3 | EN 573-3, EN 754 | A100 | |||
10.0 % Show Material materials with Elongación of 10.0 % | T3 | EN 573-3, EN 754 | A100 | |||
12.0 % Show Material materials with Elongación of 12.0 % | T3 | EN 573-3, EN 485 | A50 | |||
13.0 % Show Material materials with Elongación of 13.0 % | T3 | EN 573-3, EN 485 | A50 | |||
14.0 % Show Material materials with Elongación of 14.0 % | T3 | EN 573-3, EN 485 | A50 | |||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Wire | A10 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Tube | A10 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Tube | A10 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Tube | ||
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Módulo de cizallamiento | 27.4 GPa Show Material materials with Módulo de cizallamiento of 27.4 GPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 27.0 - 28.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 - 28.0 GPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Sheet, Strip, Tube, Wire | ||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 70.0 - 74.5 GPa Show Material materials with Módulo elástico of 70.0 - 74.5 GPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Sheet, Strip, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Resistencia a la tracción | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T3 | EN 573-3, EN 755 | |||
400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T3 | EN 573-3, EN 755 | ||||
420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T3 | EN 573-3, EN 754, EN 755 | ||||
425.0 MPa Show Material materials with Resistencia a la tracción of 425.0 MPa | T3 | EN 573-3, EN 754 | ||||
435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T3 | EN 573-3, EN 485 | ||||
440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||||
450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T3 | EN 573-3, EN 755 | ||||
20.0 °C | 400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 410.0 MPa Show Material materials with Resistencia a la tracción of 410.0 MPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 430.0 MPa Show Material materials with Resistencia a la tracción of 430.0 MPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Sheet, Strip | ||
20.0 °C | 470.0 MPa Show Material materials with Resistencia a la tracción of 470.0 MPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Rod | ||
20.0 °C | 480.0 MPa Show Material materials with Resistencia a la tracción of 480.0 MPa | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | ||
Ángulo de flexión a 180° | 4.0 °/t Show Material materials with Ángulo de flexión a 180° of 4.0 °/t | T3 | EN 573-3, EN 485 | |||
5.0 °/t Show Material materials with Ángulo de flexión a 180° of 5.0 °/t | T3 | EN 573-3, EN 485 | ||||
Ángulo de flexión a 90° | 4.0 °/t Show Material materials with Ángulo de flexión a 90° of 4.0 °/t | T3 | EN 573-3, EN 485 | |||
5.0 °/t Show Material materials with Ángulo de flexión a 90° of 5.0 °/t | T3 | EN 573-3, EN 485 | ||||
8.0 °/t Show Material materials with Ángulo de flexión a 90° of 8.0 °/t | T3 | EN 573-3, EN 485 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
20.0 °C | 875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Sheet, Strip, Tube, Wire | |
Coeficiente de dilatación térmica | -50 °C | 2.11e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.11e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | |
20 °C | 2.11e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.11e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
20 °C | 2.2899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2899999999999998e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2899999999999998e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
200 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
300 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
Conductividad térmica | 121.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 121.0 - 193.0 W/(m·K) | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire | |
Temperatura de fusión | 505.0 - 640.0 °C Show Material materials with Temperatura de fusión of 505.0 - 640.0 °C | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
505.0 - 635.0 °C Show Material materials with Temperatura de fusión of 505.0 - 635.0 °C | T3 | EN 573-3, EN 485, EN 754, EN 755 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 17000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 29000000.0 S/m | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
20.0 °C | 18000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 21000000.0 S/m | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire | |
Resistividad eléctrica | 3.45e-08 - 5.88e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 5.88e-08 Ω·m | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
4.76e-08 - 5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.56e-08 Ω·m | T3 | EN 573-3, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 3.8 - 4.9 % Show Material materials with Cobre of 3.8 - 4.9 % | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T3 | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Sheet, Strip, Tube, Wire |
0.50 % Show Material materials with Hierro of 0.50 % | T3 | EN 573-3, EN 485, EN 754, EN 755 | ||
Magnesio | 1.2 - 1.8 % Show Material materials with Magnesio of 1.2 - 1.8 % | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire |
Manganeso | 0.3 - 0.9 % Show Material materials with Manganeso of 0.3 - 0.9 % | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T3 | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Profile, Rod, Sheet, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: poor, weathering: poor | |
Workability | Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O) |