General
Property | Value | Comment |
---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | Typical for Wrought 6000 Series Aluminium |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 90.0 [-] Show Material materials with Dureza Brinell of 90.0 [-] | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Sheet | Transverse |
20.0 °C | 90.0 [-] Show Material materials with Dureza Brinell of 90.0 [-] | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod | ||
20.0 °C | 100.0 [-] Show Material materials with Dureza Brinell of 100.0 [-] | T6 | WL 3.3214-1, DIN 1725-1 | Tube | ||
Elongación | 20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging | Transverse |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging | Transverse | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Sheet | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Rod | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Sheet | Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T6 | WL 3.3214-1, DIN 1725-1 | Sheet | A50 Transverse | |
20.0 °C | 10.0 Show Material materials with Elongación of 10.0 | T6 | WL 3.3214-1, DIN 1725-1 | Tube | A50 | |
20.0 °C | 12.0 Show Material materials with Elongación of 12.0 | T6 | WL 3.3214-1, DIN 1725-1 | Tube | A50 | |
20.0 °C | 14.0 Show Material materials with Elongación of 14.0 | T6 | WL 3.3214-1, DIN 1725-1 | Tube | A50 | |
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 255.0 MPa Show Material materials with Resistencia a la tracción of 255.0 MPa | T6 | WL 3.3214-1, DIN 1725-1 | Forging | Transverse |
20.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | T6 | WL 3.3214-1, DIN 1725-1 | Forging | Transverse | |
20.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod | ||
20.0 °C | 290.0 MPa Show Material materials with Resistencia a la tracción of 290.0 MPa | T6 | WL 3.3214-1, DIN 1725-1 | Sheet | Transverse | |
20.0 °C | 290.0 MPa Show Material materials with Resistencia a la tracción of 290.0 MPa | T6 | WL 3.3214-1, DIN 1725-1 | Rod, Tube |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 887.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium |
Coeficiente de dilatación térmica | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 6000 Series Aluminium |
Conductividad térmica | 170.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 220.0 W/(m·K) | Typical for Wrought 6000 Series Aluminium |
Temperatura de fusión | 555.0 - 655.0 °C Show Material materials with Temperatura de fusión of 555.0 - 655.0 °C | Typical for Wrought 6000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 21000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium |
Resistividad eléctrica | 2.9e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.15 - 0.4 % Show Material materials with Cobre of 0.15 - 0.4 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod, Sheet, Tube |
Cromo | 0.04 - 0.35 % Show Material materials with Cromo of 0.04 - 0.35 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod, Sheet, Tube |
Hierro | 0.7 Show Material materials with Hierro of 0.7 | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod, Sheet, Tube |
Magnesio | 0.8 - 1.2 % Show Material materials with Magnesio of 0.8 - 1.2 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod, Sheet, Tube |
Manganeso | 0.15 Show Material materials with Manganeso of 0.15 | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod, Sheet, Tube |
Silicona | 0.4 - 0.8 % Show Material materials with Silicona of 0.4 - 0.8 % | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod, Sheet, Tube |
Titanio | 0.15 Show Material materials with Titanio of 0.15 | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod, Sheet, Tube |
Zinc | 0.25 Show Material materials with Zinc of 0.25 | T6 | WL 3.3214-1, DIN 1725-1 | Forging, Rod, Sheet, Tube |
Technological properties
Property | ||
---|---|---|
Workability | Excellent workability. |