General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20.0 °C | 2.8 g/cm³ Show Material materials with Densidad of 2.8 g/cm³ | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 130.0 [-] Show Material materials with Dureza Brinell of 130.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Sheet | |
20.0 °C | 140.0 [-] Show Material materials with Dureza Brinell of 140.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Rod, Tube, Sheet | ||
20.0 °C | 145.0 [-] Show Material materials with Dureza Brinell of 145.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Wire | ||
20.0 °C | 150.0 [-] Show Material materials with Dureza Brinell of 150.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile | ||
Elongación | 20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Wire | A100 |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Sheet | ||
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Sheet | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Wire | A10 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Rod | A10 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Rod, Sheet | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Tube | A10 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Tube | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Sheet | ||
Módulo de cizallamiento | 20.0 °C | 25.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 27.0 GPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | |
Módulo elástico | 20.0 °C | 70.0 - 73.0 GPa Show Material materials with Módulo elástico of 70.0 - 73.0 GPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 480.0 MPa Show Material materials with Resistencia a la tracción of 480.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Sheet | |
20.0 °C | 500.0 MPa Show Material materials with Resistencia a la tracción of 500.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Sheet, Rod | ||
20.0 °C | 510.0 MPa Show Material materials with Resistencia a la tracción of 510.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Tube, Rod | ||
20.0 °C | 520.0 MPa Show Material materials with Resistencia a la tracción of 520.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Rod | ||
20.0 °C | 530.0 MPa Show Material materials with Resistencia a la tracción of 530.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Sheet | ||
20.0 °C | 550.0 MPa Show Material materials with Resistencia a la tracción of 550.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Wire |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 862.0 J/(kg·K) Show Material materials with Calor específico of 862.0 J/(kg·K) | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | |
Coeficiente de dilatación térmica | -50.0 °C | 2.16e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.16e-05 1/K | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | |
100.0 °C | 2.34e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.34e-05 1/K | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | ||
200.0 °C | 2.43e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.43e-05 1/K | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | ||
300.0 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | ||
Conductividad térmica | 20.0 °C | 130.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 160.0 W/(m·K) | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | |
Temperatura de fusión | 465.0 - 655.0 °C Show Material materials with Temperatura de fusión of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 19000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 23000000.0 S/m | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire | |
Resistividad eléctrica | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 1.2 - 2.0 % Show Material materials with Cobre of 1.2 - 2.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Cromo | 0.18 - 0.28 % Show Material materials with Cromo of 0.18 - 0.28 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Hierro | 0.5 Show Material materials with Hierro of 0.5 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Magnesio | 2.1 - 2.9 % Show Material materials with Magnesio of 2.1 - 2.9 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Manganeso | 0.3 Show Material materials with Manganeso of 0.3 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Silicona | 0.4 Show Material materials with Silicona of 0.4 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Titanio | 0.2 Show Material materials with Titanio of 0.2 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Zinc | 5.1 - 6.1 % Show Material materials with Zinc of 5.1 - 6.1 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.4364-1 | Profile, Rod, Sheet, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |