General
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Dureza Brinell | 20.0 [-] Show Material materials with Dureza Brinell of 20.0 [-] | O | EN 573-3, EN 485, EN 755 | |||
20.0 °C | 18.0 - 26.0 [-] Show Material materials with Dureza Brinell of 18.0 - 26.0 [-] | O | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Dureza Vickers | 20.0 °C | 20.0 - 30.0 [-] Show Material materials with Dureza Vickers of 20.0 - 30.0 [-] | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | |
Elongación | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 485 | A50 | ||
22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3, EN 485, EN 755 | A50 | |||
25.0 % Show Material materials with Elongación of 25.0 % | O | EN 573-3, EN 755 | A100 | |||
26.0 % Show Material materials with Elongación of 26.0 % | O | EN 573-3, EN 485 | A50 | |||
29.0 % Show Material materials with Elongación of 29.0 % | O | EN 573-3, EN 485 | A50 | |||
32.0 % Show Material materials with Elongación of 32.0 % | O | EN 573-3, EN 485 | A100 | |||
35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A200 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A200 | |
20.0 °C | 22.0 % Show Material materials with Elongación of 22.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A200 | |
20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 40.0 % Show Material materials with Elongación of 40.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Módulo de cizallamiento | 20.0 °C | 25.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 26.5 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire, Sheet, Strip | |
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 485, EN 755 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Resistencia a la tracción | 60.0 MPa Show Material materials with Resistencia a la tracción of 60.0 MPa | O | EN 573-3, EN 755 | |||
65.0 - 105.0 MPa Show Material materials with Resistencia a la tracción of 65.0 - 105.0 MPa | O | EN 573-3, EN 485 | ||||
20.0 °C | 60.0 - 90.0 MPa Show Material materials with Resistencia a la tracción of 60.0 - 90.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | ||
20.0 °C | 60.0 - 80.0 MPa Show Material materials with Resistencia a la tracción of 60.0 - 80.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | ||
20.0 °C | 60.0 - 120.0 MPa Show Material materials with Resistencia a la tracción of 60.0 - 120.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | ||
20.0 °C | 60.0 - 100.0 MPa Show Material materials with Resistencia a la tracción of 60.0 - 100.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | ||
20.0 °C | 65.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 65.0 - 95.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 70.0 - 120.0 MPa Show Material materials with Resistencia a la tracción of 70.0 - 120.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | ||
20.0 °C | 70.0 - 100.0 MPa Show Material materials with Resistencia a la tracción of 70.0 - 100.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | ||
20.0 °C | 70.0 - 90.0 MPa Show Material materials with Resistencia a la tracción of 70.0 - 90.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 20.0 °C | 921.0 J/(kg·K) Show Material materials with Calor específico of 921.0 J/(kg·K) | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire, Sheet, Strip |
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | O | EN 573-3, EN 485, EN 755 | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | O | EN 573-3, EN 485, EN 755 | ||
Conductividad térmica | 230 W/(m·K) Show Material materials with Conductividad térmica of 230 W/(m·K) | O | EN 573-3, EN 485, EN 755 | ||
20.0 °C | 230.0 W/(m·K) Show Material materials with Conductividad térmica of 230.0 W/(m·K) | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire, Sheet, Strip | |
Temperatura de fusión | 658.0 °C Show Material materials with Temperatura de fusión of 658.0 °C | O | EN 573-3, EN 485, EN 755 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 34500000.0 - 35500000.0 S/m Show Material materials with Conductividad eléctrica of 34500000.0 - 35500000.0 S/m | O | EN 573-3, EN 485, EN 755 |
Resistividad eléctrica | 2.82e-08 - 2.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.82e-08 - 2.9e-08 Ω·m | O | EN 573-3, EN 485, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 99.5 % Show Material materials with Aluminio of 99.5 % | O | EN 573-3, EN 485, EN 755 | |
Cobre | 0.02 % Show Material materials with Cobre of 0.02 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 755 | Wire, Sheet, Strip |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire, Sheet, Strip |
0.40 % Show Material materials with Hierro of 0.40 % | O | EN 573-3, EN 485, EN 755 | ||
Magnesio | 0.05 % Show Material materials with Magnesio of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 755 | Wire, Sheet, Strip |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 755 | Wire, Sheet, Strip |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 755 | Wire, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |