General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Coil, Sheet, Strip |
Medidas
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Espesor | 0.1 mm Show Material materials with Espesor of 0.1 mm | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | 0.1 mm | Coil, Sheet, Strip |
4.0 mm Show Material materials with Espesor of 4.0 mm | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | 4.0 mm | Coil, Sheet, Strip |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 70.0 MPa Show Material materials with Bending Fatigue Strength of 70.0 MPa | O | EN 573-3, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | O | EN 573-3 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube | |
Dureza Brinell | 29.0 [-] Show Material materials with Dureza Brinell of 29.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 29.0 [-] Show Material materials with Dureza Brinell of 29.0 [-] | O | EN 573-3 | Flat | ||
20.0 °C | 30.0 [-] Show Material materials with Dureza Brinell of 30.0 [-] | O | EN 573-3 | Profile, Rod, Tube | ||
Dureza Brinell (HBW) | 29 [-] Show Material materials with Dureza Brinell (HBW) of 29 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
Elongación | 8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | |
10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
15.0 - 22.0 % Show Material materials with Elongación of 15.0 - 22.0 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A100 | ||
19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A100 | ||
22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Sheet, Strip, Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Sheet, Strip, Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3 | Sheet, Strip, Flat | A50 Transverse | |
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3 | Sheet, Strip, Flat | A50 | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3 | Sheet, Strip, Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3 | Sheet, Strip, Flat | A50 | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3 | Profile, Tube, Rod, Flat | ||
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 22.0 % Show Material materials with Elongación of 22.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 24.0 % Show Material materials with Elongación of 24.0 % | O | EN 573-3 | Flat | A50 | |
Límite elástico | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | |
35 MPa Show Material materials with Límite elástico of 35 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | ||
80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | ||
20.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Sheet, Strip, Flat | RP02 Transverse | |
20.0 °C | 35.0 MPa Show Material materials with Límite elástico of 35.0 MPa | O | EN 573-3 | Sheet, Strip, Flat | RP02 | |
20.0 °C | 40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | EN 573-3 | Profile, Rod, Tube | RP02 | |
20.0 °C | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | O | EN 573-3 | Foil | RP02 | |
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | O | EN 573-3 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | O | EN 573-3 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 90.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 90.0 - 145.0 MPa | O | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 100.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 145.0 MPa | O | EN 573-3 | Sheet, Strip, Flat | Transverse | |
20.0 °C | 100.0 - 150.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 150.0 MPa | O | EN 573-3, EN 755 | Profile, Rod, Tube, Foil, Strip, Sheet, Plate, Welded Tube, Bar | ||
20.0 °C | 100.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 145.0 MPa | O | EN 573-3, EN 1396, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Rod, Tube, Sheet, Strip, Flat, Plate, Welded Tube, Bar, Coil, Sheet, Strip | ||
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
Ángulo de flexión a 90° | 0 °/t Show Material materials with Ángulo de flexión a 90° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 897.0 J/(kg·K) Show Material materials with Calor específico of 897.0 J/(kg·K) | O | EN 573-3 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube | |
Coeficiente de dilatación térmica | 20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | 20-100°C | |
Conductividad térmica | 200 W/(m·K) Show Material materials with Conductividad térmica of 200 W/(m·K) | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
201 W/(m·K) Show Material materials with Conductividad térmica of 201 W/(m·K) | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
20.0 °C | 201.0 W/(m·K) Show Material materials with Conductividad térmica of 201.0 W/(m·K) | O | EN 573-3 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube | ||
Temperatura de fusión | 630.0 - 655.0 °C Show Material materials with Temperatura de fusión of 630.0 - 655.0 °C | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 30000000.0 S/m Show Material materials with Conductividad eléctrica of 30000000.0 S/m | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
Resistividad eléctrica | 3.33e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.33e-08 Ω·m | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 3.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-08 Ω·m | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Coil, Sheet, Strip |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | O | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Cobre of 0.2 % | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar | |
0.2 % Show Material materials with Cobre of 0.2 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar |
0.1 % Show Material materials with Cromo of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Hierro | 0.45 % Show Material materials with Hierro of 0.45 % | O | EN 573-3 | Rod, Tube |
0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-3 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube | |
0.70 % Show Material materials with Hierro of 0.70 % | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
0.7 % Show Material materials with Hierro of 0.7 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Magnesio | 0.5 - 1.1 % Show Material materials with Magnesio of 0.5 - 1.1 % | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar, Coil, Sheet, Strip |
0.7 - 1.1 % Show Material materials with Magnesio of 0.7 - 1.1 % | O | EN 573-3 | Rod, Tube | |
Manganeso | 0.15 % Show Material materials with Manganeso of 0.15 % | O | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Manganeso of 0.2 % | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar | |
0.2 % Show Material materials with Manganeso of 0.2 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar |
0.3 % Show Material materials with Silicona of 0.3 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | O | EN 573-3 | Rod, Tube |
0.25 % Show Material materials with Zinc of 0.25 % | O | EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755 | Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar | |
0.25 % Show Material materials with Zinc of 0.25 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Heat exchangers: Fins, General applications; Cosmetics: Cosmetics pieces; Automotive trim: Interior trim; Components: Automotive fins, Heat exchangers | |
Brazing | hard brazing (with flux/ without flux): acceptable / sufficient, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (O) |