General
Property | Value | Comment |
---|---|---|
Densidad | 2.75 - 2.84 g/cm³ Show Material materials with Densidad of 2.75 - 2.84 g/cm³ | Typical for Wrought 2000 Series Aluminium |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 130.0 [-] Show Material materials with Dureza Brinell of 130.0 [-] | T6 | WL 3.1254-1 | Forging | Transverse |
20.0 °C | 130.0 [-] Show Material materials with Dureza Brinell of 130.0 [-] | T6 | WL 3.1254-1 | Forging | ||
Elongación | 20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | T6 | WL 3.1254-1 | Forging | Transverse |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T6 | WL 3.1254-1 | Forging | ||
Límite elástico | 20.0 °C | 350.0 MPa Show Material materials with Límite elástico of 350.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 Transverse |
20.0 °C | 350.0 MPa Show Material materials with Límite elástico of 350.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 | |
20.0 °C | 360.0 MPa Show Material materials with Límite elástico of 360.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 Transverse | |
20.0 °C | 360.0 - 385.0 MPa Show Material materials with Límite elástico of 360.0 - 385.0 MPa | T6 | WL 3.1254-1 | |||
20.0 °C | 360.0 MPa Show Material materials with Límite elástico of 360.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 | |
20.0 °C | 365.0 MPa Show Material materials with Límite elástico of 365.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 Transverse | |
20.0 °C | 365.0 MPa Show Material materials with Límite elástico of 365.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 | |
20.0 °C | 370.0 MPa Show Material materials with Límite elástico of 370.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 Transverse | |
20.0 °C | 370.0 MPa Show Material materials with Límite elástico of 370.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 | |
20.0 °C | 380.0 MPa Show Material materials with Límite elástico of 380.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 Transverse | |
20.0 °C | 380.0 MPa Show Material materials with Límite elástico of 380.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 | |
20.0 °C | 385.0 MPa Show Material materials with Límite elástico of 385.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 Transverse | |
20.0 °C | 385.0 MPa Show Material materials with Límite elástico of 385.0 MPa | T6 | WL 3.1254-1 | Forging | RP02 | |
Módulo de cizallamiento | 26.0 - 27.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Módulo elástico | 70.0 - 73.0 GPa Show Material materials with Módulo elástico of 70.0 - 73.0 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 20.0 °C | 18.3 - 30.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.3 - 30.6 MPa·√m | T6 | WL 3.1254-1 | ||
20.0 °C | 18.3 - 19.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.3 - 19.1 MPa·√m | T6 | WL 3.1254-1 | |||
20.0 °C | 18.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.3 MPa·√m | T6 | WL 3.1254-1 | |||
20.0 °C | 19.1 - 30.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.1 - 30.6 MPa·√m | T6 | WL 3.1254-1 | |||
20.0 °C | 19.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 19.1 MPa·√m | T6 | WL 3.1254-1 | |||
20.0 °C | 30.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.6 MPa·√m | T6 | WL 3.1254-1 | |||
Resistencia a la tracción | 20.0 °C | 395.0 MPa Show Material materials with Resistencia a la tracción of 395.0 MPa | T6 | WL 3.1254-1 | Forging | |
20.0 °C | 400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 405.0 MPa Show Material materials with Resistencia a la tracción of 405.0 MPa | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 405.0 MPa Show Material materials with Resistencia a la tracción of 405.0 MPa | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 415.0 MPa Show Material materials with Resistencia a la tracción of 415.0 MPa | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 415.0 MPa Show Material materials with Resistencia a la tracción of 415.0 MPa | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 420.0 MPa Show Material materials with Resistencia a la tracción of 420.0 MPa | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 425.0 MPa Show Material materials with Resistencia a la tracción of 425.0 MPa | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 425.0 MPa Show Material materials with Resistencia a la tracción of 425.0 MPa | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 435.0 MPa Show Material materials with Resistencia a la tracción of 435.0 MPa | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T6 | WL 3.1254-1 | Forging | ||
20.0 °C | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T6 | WL 3.1254-1 | Forging | Transverse | |
20.0 °C | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T6 | WL 3.1254-1 | Forging |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 816.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Coeficiente de dilatación térmica | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Conductividad térmica | 112.0 - 251.0 W/(m·K) Show Material materials with Conductividad térmica of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Temperatura de fusión | 500.0 - 650.0 °C Show Material materials with Temperatura de fusión of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 30000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
Resistividad eléctrica | 3.4e-08 - 6e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 3.9 - 5.0 % Show Material materials with Cobre of 3.9 - 5.0 % | T6 | WL 3.1254-1 | Forging |
Cromo | 0.1 Show Material materials with Cromo of 0.1 | T6 | WL 3.1254-1 | Forging |
Hierro | 0.3 Show Material materials with Hierro of 0.3 | T6 | WL 3.1254-1 | Forging |
Magnesio | 0.2 - 0.8 % Show Material materials with Magnesio of 0.2 - 0.8 % | T6 | WL 3.1254-1 | Forging |
Manganeso | 0.4 - 1.2 % Show Material materials with Manganeso of 0.4 - 1.2 % | T6 | WL 3.1254-1 | Forging |
Silicona | 0.5 - 1.2 % Show Material materials with Silicona of 0.5 - 1.2 % | T6 | WL 3.1254-1 | Forging |
Titanio | 0.15 Show Material materials with Titanio of 0.15 | T6 | WL 3.1254-1 | Forging |
Zinc | 0.25 Show Material materials with Zinc of 0.25 | T6 | WL 3.1254-1 | Forging |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |