General
Property | Value | Comment |
---|---|---|
Densidad | 2.7 - 2.85 g/cm³ Show Material materials with Densidad of 2.7 - 2.85 g/cm³ | Typical for Wrought 7000 Series Aluminium |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 140.0 [-] Show Material materials with Dureza Brinell of 140.0 [-] | T74 | WL 3.4354-1 | Forging, Rod | Transverse |
20.0 °C | 140.0 [-] Show Material materials with Dureza Brinell of 140.0 [-] | T74 | WL 3.4354-1 | Forging, Rod, Profile | ||
Elongación | 20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T74 | WL 3.4354-1 | Forging | Transverse |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T74 | WL 3.4354-1 | Forging | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T74 | WL 3.4354-1 | Forging, Rod, Profile | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T74 | WL 3.4354-1 | Profile, Forging | ||
Módulo de cizallamiento | 26.4 - 27.1 GPa Show Material materials with Módulo de cizallamiento of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Módulo elástico | 69.0 - 72.0 GPa Show Material materials with Módulo elástico of 69.0 - 72.0 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 20.0 °C | 22.0 - 38.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 38.0 MPa·√m | T74 | WL 3.4354-1 | Rod | |
20.0 °C | 22.0 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 29.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 22.0 - 36.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 36.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 22.0 - 25.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 25.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 22.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 22.0 - 42.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 42.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 22.0 - 28.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 28.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 24.0 - 31.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 31.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 24.0 - 32.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 32.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 24.0 - 26.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 26.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 24.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 25.0 - 40.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.0 - 40.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 25.0 - 28.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.0 - 28.0 MPa·√m | T74 | WL 3.4354-1 | Forging, Rod | ||
20.0 °C | 25.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.0 MPa·√m | T74 | WL 3.4354-1 | Forging, Rod | ||
20.0 °C | 25.0 - 26.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.0 - 26.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 25.0 - 38.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.0 - 38.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 25.0 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.0 - 29.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 25.0 - 36.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.0 - 36.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 25.0 - 42.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.0 - 42.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 26.0 - 31.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.0 - 31.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 26.0 - 32.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.0 - 32.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 26.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 26.0 - 40.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.0 - 40.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 26.0 - 28.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.0 - 28.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 28.0 - 40.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.0 - 40.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 28.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.0 MPa·√m | T74 | WL 3.4354-1 | Forging, Rod | ||
20.0 °C | 28.0 - 38.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.0 - 38.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 28.0 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.0 - 29.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 28.0 - 36.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.0 - 36.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 28.0 - 42.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.0 - 42.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 29.0 - 38.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 38.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 29.0 - 36.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 36.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 29.0 - 42.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 42.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 31.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 31.0 - 32.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.0 - 32.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 32.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 32.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 36.0 - 38.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 36.0 - 38.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 36.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 36.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 36.0 - 42.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 36.0 - 42.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 38.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 38.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 38.0 - 42.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 38.0 - 42.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
20.0 °C | 40.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 40.0 MPa·√m | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 42.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 42.0 MPa·√m | T74 | WL 3.4354-1 | Rod | ||
Resistencia a la tracción | 20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T74 | WL 3.4354-1 | Forging | Transverse |
20.0 °C | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T74 | WL 3.4354-1 | Forging | Transverse | |
20.0 °C | 460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T74 | WL 3.4354-1 | Forging, Rod | Transverse | |
20.0 °C | 460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 470.0 MPa Show Material materials with Resistencia a la tracción of 470.0 MPa | T74 | WL 3.4354-1 | Forging, Rod | Transverse | |
20.0 °C | 470.0 MPa Show Material materials with Resistencia a la tracción of 470.0 MPa | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 480.0 MPa Show Material materials with Resistencia a la tracción of 480.0 MPa | T74 | WL 3.4354-1 | Forging | Transverse | |
20.0 °C | 480.0 MPa Show Material materials with Resistencia a la tracción of 480.0 MPa | T74 | WL 3.4354-1 | Forging | ||
20.0 °C | 490.0 MPa Show Material materials with Resistencia a la tracción of 490.0 MPa | T74 | WL 3.4354-1 | Forging | Transverse | |
20.0 °C | 500.0 MPa Show Material materials with Resistencia a la tracción of 500.0 MPa | T74 | WL 3.4354-1 | Forging | Transverse | |
20.0 °C | 500.0 MPa Show Material materials with Resistencia a la tracción of 500.0 MPa | T74 | WL 3.4354-1 | Profile, Forging | ||
20.0 °C | 510.0 MPa Show Material materials with Resistencia a la tracción of 510.0 MPa | T74 | WL 3.4354-1 | Forging, Profile, Rod | ||
20.0 °C | 530.0 MPa Show Material materials with Resistencia a la tracción of 530.0 MPa | T74 | WL 3.4354-1 | Rod |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 795.0 - 1050.0 J/(kg·K) Show Material materials with Calor específico of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium |
Coeficiente de dilatación térmica | 2.1e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 - 2.4e-05 1/K | Typical for Wrought 7000 Series Aluminium |
Conductividad térmica | 121.0 - 170.0 W/(m·K) Show Material materials with Conductividad térmica of 121.0 - 170.0 W/(m·K) | Typical for Wrought 7000 Series Aluminium |
Temperatura de fusión | 465.0 - 655.0 °C Show Material materials with Temperatura de fusión of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 34000000.0 S/m | Typical for Wrought 7000 Series Aluminium |
Resistividad eléctrica | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.6 - 1.3 % Show Material materials with Cobre of 0.6 - 1.3 % | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Cromo | 0.1 - 0.25 % Show Material materials with Cromo of 0.1 - 0.25 % | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Hierro | 0.2 Show Material materials with Hierro of 0.2 | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Magnesio | 2.1 - 2.9 % Show Material materials with Magnesio of 2.1 - 2.9 % | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Manganeso | 0.1 Show Material materials with Manganeso of 0.1 | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Plata | 0.25 - 0.4 % Show Material materials with Plata of 0.25 - 0.4 % | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Silicona | 0.2 Show Material materials with Silicona of 0.2 | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Titanio | 0.2 Show Material materials with Titanio of 0.2 | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Zinc | 5.5 - 6.5 % Show Material materials with Zinc of 5.5 - 6.5 % | T74 | WL 3.4354-1 | Forging, Profile, Rod |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |